CO catalyst as well as preparation method and application thereof
By preparing CO catalysts containing platinum and rare earth oxides, the problem of low CO removal efficiency in the prior art is solved, and efficient removal and long-life catalysts under medium temperature conditions are achieved. It is suitable for the treatment of CO in sintered flue gas in the steel industry. .
Patent Information
- Application Number
- CN202411151196.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art has poor effect on carbon monoxide (CO) removal in desulfurization and denitrification devices, and the existing catalysts release a large amount of heat energy when oxidizing CO under medium and low temperature conditions, affecting the efficiency of the device.
Using a CO catalyst preparation method, the catalyst obtained is soaked and roasted by ball milling a mixed slurry of platinum precursor, titanium dioxide, rare earth oxides, transition metal oxides, binders and dispersants, so as to be efficient under medium temperature conditions. Remove CO and extend the life of the catalyst.
It achieves efficient removal of CO under medium temperature conditions, the catalyst has a long service life, and the removal efficiency of CO at a temperature of 230-280°C reaches more than 80%.
Smart Images

Figure CN119034729A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a CO catalyst and a preparation method and application thereof. Background Art
[0002] Sintering flue gas contains dust, SO x 、NO x The dust removal and desulfurization and denitrification devices can effectively remove dust, SO x and NO x , but the removal effect of CO is poor. CO can cause photochemical pollution, reduce ozone content, pollute the environment, damage the human respiratory system and nervous system, and seriously endanger human health. The prior art proposes to add a CO catalytic oxidation device between the desulfurization device and the SCR denitrification device to oxidize CO under medium and low temperature conditions while releasing a large amount of heat energy to provide heat energy for the back-end SCR.
[0003] CN117839773A discloses an integral carbon monoxide catalyst, comprising a carrier and metal catalytic particles loaded on the surface of the carrier. The loading amount of the metal catalytic particles is 90-150 kg / m 3 The metal catalytic particles include one or more of titanium particles, cerium particles, cobalt particles, nickel particles, ruthenium particles, rhodium particles, palladium particles, iridium particles, platinum particles, and molybdenum particles. The carrier includes one or more of cordierite, honeycomb, and hierarchical porous carbon. The catalyst has a low removal efficiency for CO.
[0004] CN114643065A discloses a noble metal catalyst for catalytic oxidation of CO, wherein the surface of TiO2 is loaded with noble metal and auxiliary agent, the catalyst carrier is TiO2, the active component of the catalyst is one or more of the noble metals Pt, Ag, Pd, Rh, Ir, Ru, Os or Au; the auxiliary agent is one or more of the noble metals Co, Cr, Zr, Sn, Mo, W, Fe, Ce, Ni, Nb; the TiO2 is 78-98.9wt%, the noble metal is 0.1-2wt%, and the auxiliary agent is 1-20wt%. The operating temperature of the catalyst is relatively low. Summary of the invention
[0005] In view of this, an object of the present invention is to provide a method for preparing a CO catalyst, wherein the CO catalyst prepared by the method has a high removal efficiency for CO under medium temperature conditions. Furthermore, the CO catalyst prepared by the method has a long service life. Another object of the present invention is to provide a CO catalyst. Still another object of the present invention is to provide a use of a CO catalyst.
[0006] The above purpose is achieved through the following technical solutions.
[0007] In one aspect, the present invention provides a method for preparing a CO catalyst, comprising the following steps:
[0008] (1) ball-milling a mixed slurry containing 1 to 20 parts by weight of a platinum precursor, 600 to 1500 parts by weight of titanium dioxide, 15 to 110 parts by weight of a rare earth oxide, 10 to 30 parts by weight of a transition metal oxide, 150 to 1400 parts by weight of a binder and 4 to 18 parts by weight of a dispersant to obtain a ball-milled slurry;
[0009] Wherein, the rare earth oxide is selected from one or more of lanthanum oxide, cerium oxide, and praseodymium oxide; the transition metal oxide is selected from one or more of zirconium oxide and iridium oxide; the binder is selected from one or more of aluminum sol, silica sol, and polyethylene glycol; the dispersant is selected from one or more of polyethylene oxide, hydroxypropyl methylcellulose, and polyethylene glycol;
[0010] (2) placing the carrier in the ball mill slurry, immersing for 1 to 8 minutes and then taking it out to obtain a carrier loaded with the slurry; blowing the carrier loaded with the slurry until no slurry drips, and then drying to obtain a dry loaded carrier; calcining the dry loaded carrier to obtain a CO catalyst;
[0011] Wherein, the carrier is selected from one or more of cordierite, glass fiber corrugated board, and titanium dioxide.
[0012] According to the preparation method of the present invention, preferably, the mixed slurry further contains 3000 to 5300 parts by weight of water.
[0013] According to the preparation method of the present invention, preferably, the rare earth oxide is selected from the following compositions:
[0014] (A) lanthanum oxide and cerium oxide;
[0015] (B) cerium oxide and praseodymium oxide;
[0016] (C) Cerium oxide.
[0017] According to the preparation method of the present invention, preferably, the binder is selected from one of the following compositions:
[0018] (A) Polyethylene glycol and aluminum sol;
[0019] (B) polyethylene glycol, aluminum sol and silica sol;
[0020] (C) Aluminum sol and silica sol;
[0021] (D) Aluminum sol.
[0022] According to the preparation method of the present invention, preferably, the dispersant is selected from one of the following compositions:
[0023] (A) Polyethylene oxide;
[0024] (B) Hydroxypropyl methylcellulose;
[0025] (C) Polyethylene oxide and polyethylene glycol.
[0026] According to the preparation method of the present invention, preferably, ball milling is carried out under the condition that the rotation speed is 100 - 600 rpm, and the ball milling time is 1.5 - 4.5 h.
[0027] According to the preparation method of the present invention, preferably, the drying temperature is 100 - 150 °C, and the drying time is 7 - 20 h; the calcination temperature is 400 - 600 °C, and the calcination time is 3 - 8 h.
[0028] On the other hand, the present invention provides a CO catalyst, which is prepared by the above - mentioned preparation method.
[0029] On still another aspect, the present invention provides the use of the above - mentioned CO catalyst in the catalytic oxidation of carbon monoxide.
[0030] According to the use of the present invention, preferably, the carbon monoxide exists in a gaseous substance, the concentration of the carbon monoxide is 3000 - 8000 ppm, and the use temperature of the carbon monoxide catalyst is 230 - 280 °C.
[0031] The CO catalyst obtained by the preparation method of the present invention has a high removal efficiency for CO and a long service life. Description of the Drawings
[0032] Figure 1 It is a graph of the CO removal efficiency of the catalysts in Examples 1 - 5. Detailed Description of the Invention
[0033] The following is a further description of the present invention with reference to specific examples, but the protection scope of the present invention is not limited thereto.
[0034] <Preparation Method of CO Catalyst>
[0035] The preparation method of the CO catalyst of the present invention includes the following steps: (1) a step of preparing a slurry; and (2) a step of loading.
[0036] Steps for preparing slurry
[0037] Ball - mill a mixed slurry containing a platinum precursor, titanium dioxide, rare - earth oxide, transition - metal oxide, binder and dispersant to obtain a ball - milled slurry.
[0038] The dosage of the platinum precursor is 1 - 20 parts by weight; preferably 3 - 15 parts by weight; more preferably 3 - 6 parts by weight. The platinum precursor can be chloroplatinic acid.
[0039] The amount of titanium dioxide used is 600 to 1500 parts by weight, preferably 700 to 1200 parts by weight, and more preferably 780 to 800 parts by weight.
[0040] The amount of rare earth oxide used is 15 to 110 parts by weight, preferably 20 to 100 parts by weight, and more preferably 90 to 96 parts by weight.
[0041] The rare earth oxide is selected from one or more of lanthanum oxide, cerium oxide and praseodymium oxide.
[0042] In some embodiments, the rare earth oxide is a combination of lanthanum oxide and cerium oxide. The amount of lanthanum oxide can be 25 to 80 parts by weight. In some embodiments, the amount of lanthanum oxide is 28 to 35 parts by weight. In other embodiments, the amount of lanthanum oxide is 68 to 72 parts by weight. The amount of cerium oxide can be 4 to 30 parts by weight. In some embodiments, the amount of cerium oxide is 6 to 8 parts by weight. In other embodiments, the amount of cerium oxide is 24 to 26 parts by weight.
[0043] In certain embodiments, the rare earth oxide is a combination of cerium oxide and praseodymium oxide. The amount of cerium oxide can be 60 to 85 parts by weight, preferably 65 to 80 parts by weight, and more preferably 72 to 75 parts by weight. The amount of praseodymium oxide can be 15 to 35 parts by weight, preferably 20 to 30 parts by weight, and more preferably 24 to 26 parts by weight.
[0044] In some embodiments, the rare earth oxide is cerium oxide. The amount of cerium oxide used can be 15 to 35 parts by weight, preferably 20 to 30 parts by weight, and more preferably 24 to 26 parts by weight.
[0045] The transition metal oxide is selected from one or more of zirconium oxide and iridium oxide. In some embodiments, the transition metal oxide is zirconium oxide. In other embodiments, the transition metal oxide is iridium oxide. An appropriate amount of iridium oxide combined with other ingredients can better improve the removal efficiency and service life of the catalyst for CO.
[0046] The amount of transition metal oxide used is 10 to 30 parts by weight, preferably 15 to 25 parts by weight, and more preferably 20 to 24 parts by weight.
[0047] The amount of the binder is 150 to 1400 parts by weight. In some embodiments, the amount of the binder is 180 to 200 parts by weight. In other embodiments, the amount of the binder is 800 to 1000 parts by weight. In still other embodiments, the amount of the binder is 1100 to 1300 parts by weight.
[0048] The binder is selected from one or more of aluminum sol, silica sol and polyethylene glycol. The molecular weight of polyethylene glycol is 10,000 to 30,000, preferably 15,000 to 25,000.
[0049] In some embodiments, the binder is a combination of polyethylene glycol and aluminum sol. The amount of polyethylene glycol used can be 550 to 750 parts by weight, preferably 650 to 700 parts by weight. The amount of aluminum sol used can be 100 to 250 parts by weight, preferably 150 to 220 parts by weight, and more preferably 180 to 200 parts by weight.
[0050] In other embodiments, the binder is a combination of polyethylene glycol, aluminum sol and silica sol. The amount of polyethylene glycol can be 600 to 800 parts by weight, preferably 650 to 750 parts by weight, and more preferably 700 to 720 parts by weight. The amount of aluminum sol can be 80 to 150 parts by weight, preferably 100 to 120 parts by weight. The amount of silica sol can be 80 to 150 parts by weight, preferably 100 to 120 parts by weight.
[0051] In some other embodiments, the binder is a combination of aluminum sol and silica sol. The amount of aluminum sol used can be 800 to 1000 parts by weight, preferably 900 to 950 parts by weight. The amount of silica sol used is 200 to 400 parts by weight, preferably 300 to 350 parts by weight.
[0052] In some other embodiments, the binder is aluminum sol. The amount of aluminum sol used can be 130 to 250 parts by weight, preferably 180 to 200 parts by weight.
[0053] The amount of the dispersant used is 4 to 18 parts by weight, preferably 5 to 12 parts by weight, and more preferably 6 to 7 parts by weight.
[0054] The dispersant is selected from one or more of polyethylene oxide, hydroxypropyl methylcellulose and polyethylene glycol. The molecular weight of polyethylene glycol may be 800 to 3000, preferably 1000 to 2000.
[0055] In certain embodiments, the dispersant is polyethylene oxide, and the amount of polyethylene oxide used can be 5 to 10 parts by weight, preferably 7 to 8 parts by weight.
[0056] In certain embodiments, the dispersant is hydroxypropyl methylcellulose, and the amount of hydroxypropyl methylcellulose used can be 3 to 8 parts by weight, preferably 5 to 6 parts by weight.
[0057] In certain embodiments, the dispersant is polyethylene oxide and polyethylene glycol. The amount of polyethylene oxide can be 3 to 8 parts by weight, preferably 5 to 6 parts by weight. The amount of polyethylene glycol can be 3 to 8 parts by weight, preferably 5 to 6 parts by weight.
[0058] The mixed slurry of the present invention further contains water. The amount of water used is 3000 to 5300 parts by weight; preferably 3500 to 5100 parts by weight; more preferably 4900 to 5000 parts by weight.
[0059] Ball milling is carried out at a rotational speed of 100 to 600 rpm; preferably 200 to 300 rpm.
[0060] The ball milling time can be 1.5 to 4.5 h; preferably 3 to 4 h.
[0061] Load Steps
[0062] The carrier is placed in the ball-milled slurry, taken out after impregnation for 1 to 8 min to obtain a carrier loaded with the slurry; the carrier loaded with the slurry is blown until no slurry drips, and then dried to obtain a dried loaded carrier; the dried loaded carrier is calcined to obtain a CO catalyst.
[0063] The carrier is selected from one or more of cordierite, fiberglass corrugated board, and titanium dioxide. Preferably, the carrier is titanium dioxide. Such a carrier cooperates with the active components in the slurry, which can improve the removal efficiency of the catalyst for CO and extend the service life of the catalyst.
[0064] The impregnation time of the carrier in the ball-milled slurry is 1 to 8 min; preferably 2 to 5 min; more preferably 3 to 4 min.
[0065] The drying temperature can be 100 to 150 °C; preferably 110 to 120 °C. The drying time can be 7 to 20 h; preferably 10 to 15 h. Drying can be carried out in a tunnel drying furnace.
[0066] The calcination temperature can be 400 to 600 °C; preferably 450 to 550 °C. The calcination time can be 3 to 8 h; preferably 4 to 5 h. Calcination can be carried out in a calcination furnace.
[0067] The heating rate from the initial temperature to the calcination temperature can be 2 to 10 °C / min; preferably 5 to 7 °C / min.
[0068] <CO Catalyst and Its Use>
[0069] The CO catalyst of the present invention is prepared by the above method. The CO catalyst of the present invention has a high removal efficiency and service life for CO. Therefore, the present invention provides the use of the above CO catalyst in the catalytic oxidation of carbon monoxide.
[0070] Carbon monoxide can exist in gaseous substances. The gaseous substance can be the sintering flue gas in the iron and steel industry.
[0071] The concentration of carbon monoxide in the gaseous substance may be 3000 to 8000 ppm, preferably 4000 to 7000 ppm, and more preferably 5000 to 6000 ppm.
[0072] The operating temperature of the CO catalyst may be 230 to 280°C, preferably 250 to 270°C, and more preferably 260 to 270°C.
[0073] The airspeed can be 15000~25000h -1 ; preferably 18000~23000h -1 More preferably, 20000 to 21000 hours -1 .
[0074] Example 1
[0075] 15 g of chloroplatinic acid, 846 g of titanium dioxide, 31.2 g of lanthanum oxide, 7.2 g of cerium oxide, 15.6 g of zirconium oxide, 672 g of polyethylene glycol (molecular weight 20,000), 180 g of aluminum sol, 7.8 g of polyethylene oxide and 4220.7 g of distilled water were uniformly mixed to obtain a mixed slurry, and the mixed slurry was ball-milled in a ball mill at a rotation speed of 500 rpm for 2.5 h to obtain a ball-milled slurry.
[0076] The cordierite carrier was placed in the ball mill slurry, immersed for 5 minutes and then taken out to obtain a carrier loaded with slurry. The carrier loaded with slurry was purged with compressed air until no slurry dripped, and then dried in a tunnel drying furnace at 110°C for 12 hours to obtain a dry loaded carrier. The dry loaded carrier was calcined in a calcining furnace at 500°C for 5 hours to obtain a CO catalyst. The heating rate from the initial temperature to 500°C was 5°C / min.
[0077] The CO catalyst was placed in the reactor at a temperature of 270 °C and a space velocity of 20000 h -1 The concentration of CO in the flue gas to be treated is 5000ppm. The CO removal efficiency is calculated as follows: Figure 1 As shown. Figure 1 It can be seen that after the CO catalyst of this embodiment is used for 281 minutes, the CO removal efficiency can reach more than 80%.
[0078] Example 2
[0079] 6 g of chloroplatinic acid, 1380 g of titanium dioxide, 72 g of lanthanum oxide, 24 g of cerium oxide, 24 g of zirconium oxide, 672 g of polyethylene glycol (molecular weight 20,000), 180 g of aluminum sol, 7.8 g of polyethylene oxide and 3634.2 g of distilled water were uniformly mixed to obtain a mixed slurry. The mixed slurry was ball-milled in a ball mill at a rotation speed of 500 rpm for 2.5 hours to obtain a ball-milled slurry.
[0080] The glass fiber corrugated plate carrier was placed in the ball mill slurry, immersed for 5 minutes and then taken out to obtain a carrier loaded with slurry. The carrier loaded with slurry was purged with compressed air until no slurry dripped, and then dried in a tunnel drying furnace at 110°C for 12 hours to obtain a dry loaded carrier. The dry loaded carrier was calcined in a calcining furnace at 500°C for 5 hours to obtain a CO catalyst. The heating rate from the initial temperature to 500°C was 5°C / min.
[0081] The CO catalyst was placed in the reactor at a temperature of 260 °C and a space velocity of 20000 h -1 The concentration of CO in the flue gas to be treated is 5000ppm. The CO removal efficiency is calculated as follows: Figure 1 As shown. Figure 1 It can be seen that after the CO catalyst of this embodiment is used for 281 minutes, the CO removal efficiency can reach about 80%.
[0082] Example 3
[0083] 3g of chloroplatinic acid, 1380g of titanium dioxide, 72g of cerium oxide, 24g of zirconium oxide, 24g of praseodymium oxide, 720g of polyethylene glycol (molecular weight 20000), 120g of aluminum sol, 120g of silica sol, 6g of hydroxypropyl methylcellulose and 3531g of distilled water were uniformly mixed to obtain a mixed slurry. The mixed slurry was ball-milled in a ball mill at a rotation speed of 500rpm for 3.5h to obtain a ball-milled slurry.
[0084] The glass fiber corrugated plate carrier was placed in the ball mill slurry, immersed for 2 minutes and then taken out to obtain a carrier loaded with slurry. The carrier loaded with slurry was purged with compressed air until no slurry dripped, and then dried in a tunnel drying furnace at 110°C for 12 hours to obtain a dry loaded carrier. The dry loaded carrier was calcined in a calcining furnace at 500°C for 5 hours to obtain a CO catalyst. The heating rate from the initial temperature to 500°C was 5°C / min.
[0085] The CO catalyst was placed in the reactor at a temperature of 240 °C and a space velocity of 20000 h -1The concentration of CO in the flue gas to be treated is 5000ppm. The CO removal efficiency is calculated as follows: Figure 1 As shown. Figure 1 It can be seen that after the CO catalyst of this embodiment is used for 281 minutes, the CO removal efficiency can reach about 60%.
[0086] Example 4
[0087] 3 g of chloroplatinic acid, 780 g of titanium dioxide, 72 g of lanthanum oxide, 24 g of cerium oxide, 24 g of iridium oxide, 180 g of aluminum sol, 6 g of hydroxypropyl methylcellulose and 4932 g of distilled water were uniformly mixed to obtain a mixed slurry, and the mixed slurry was ball-milled in a ball mill at a rotation speed of 200 rpm for 3 hours to obtain a ball-milled slurry.
[0088] The titanium dioxide carrier was placed in the ball mill slurry, immersed for 3 minutes and then taken out to obtain a carrier loaded with slurry. The carrier loaded with slurry was purged with compressed air until no slurry dripped, and then dried in a tunnel drying furnace at 110°C for 12 hours to obtain a dry loaded carrier. The dry loaded carrier was calcined in a calcining furnace at 500°C for 5 hours to obtain a CO catalyst. The heating rate from the initial temperature to 500°C was 5°C / min.
[0089] The CO catalyst was placed in the reactor at a temperature of 260 °C and a space velocity of 20000 h -1 The concentration of CO in the flue gas to be treated is 5000ppm. The CO removal efficiency is calculated as follows: Figure 1 As shown. Figure 1 It can be seen that after the CO catalyst of this embodiment is used for 281 minutes, the CO removal efficiency is close to 100%.
[0090] Example 5
[0091] 6 g of chloroplatinic acid, 1176 g of titanium dioxide, 24 g of cerium oxide, 24 g of iridium oxide, 900 g of aluminum sol, 300 g of silica sol, 6 g of polyethylene oxide, 6 g of polyethylene glycol (molecular weight 1500) and 3582 g of distilled water were uniformly mixed to obtain a mixed slurry. The mixed slurry was ball-milled in a ball mill at a rotation speed of 300 rpm for 2.5 hours to obtain a ball-milled slurry.
[0092] The titanium dioxide carrier was placed in the ball mill slurry, immersed for 3 minutes and then taken out to obtain a carrier loaded with slurry. The carrier loaded with slurry was purged with compressed air until no slurry dripped, and then dried in a tunnel drying furnace at 110°C for 12 hours to obtain a dry loaded carrier. The dry loaded carrier was calcined in a calcining furnace at 500°C for 5 hours to obtain a CO catalyst. The heating rate from the initial temperature to 500°C was 5°C / min.
[0093] The CO catalyst was placed in the reactor at a temperature of 260 °C and a space velocity of 20000 h -1 The concentration of CO in the flue gas to be treated is 5000ppm. The CO removal efficiency is calculated as follows: Figure 1 As shown. Figure 1 It can be seen that after the CO catalyst of this embodiment is used for 281 minutes, the CO removal efficiency is above 95%.
[0094] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.
Claims
1. A method for preparing a CO catalyst, characterized in that: The steps include: (1) ball-milling a mixed slurry containing 1 to 20 parts by weight of a platinum precursor, 600 to 1500 parts by weight of titanium dioxide, 15 to 110 parts by weight of a rare earth oxide, 10 to 30 parts by weight of a transition metal oxide, 150 to 1400 parts by weight of a binder and 4 to 18 parts by weight of a dispersant to obtain a ball-milled slurry; Wherein, the rare earth oxide is selected from one or more of lanthanum oxide, cerium oxide, and praseodymium oxide; the transition metal oxide is selected from one or more of zirconium oxide and iridium oxide; the binder is selected from one or more of aluminum sol, silica sol, and polyethylene glycol; the dispersant is selected from one or more of polyethylene oxide, hydroxypropyl methylcellulose, and polyethylene glycol; (2) placing the carrier in the ball mill slurry, immersing for 1 to 8 minutes and then taking it out to obtain a carrier loaded with the slurry; blowing the carrier loaded with the slurry until no slurry drips, and then drying to obtain a dry loaded carrier; calcining the dry loaded carrier to obtain a CO catalyst; Wherein, the carrier is selected from one or more of cordierite, glass fiber corrugated board, and titanium dioxide.
2. The preparation method according to claim 1, characterized in that: The mixed slurry also contains 3000 to 5300 parts by weight of water.
3. The preparation method according to claim 1, characterized in that: The rare earth oxide is selected from the following compositions: (A) lanthanum oxide and cerium oxide; (B) cerium oxide and praseodymium oxide; (C) Cerium oxide.
4. The preparation method according to claim 1, characterized in that: The binder is selected from the following compositions: (A) Polyethylene glycol and aluminum sol; (B) polyethylene glycol, aluminum sol and silica sol; (C) Aluminum sol and silica sol; (D) Aluminum sol.
5. The preparation method according to claim 1, characterized in that: The dispersant is selected from the following compositions: (A) polyethylene oxide; (B) Hydroxypropyl methylcellulose; (C) Polyethylene oxide and polyethylene glycol.
6. The preparation method according to claim 1, characterized in that: The ball milling is carried out at a rotation speed of 100 to 600 rpm, and the ball milling time is 1.5 to 4.5 hours.
7. The preparation method according to claim 1, characterized in that: The drying temperature is 100-150°C, and the drying time is 7-20 hours; the roasting temperature is 400-600°C, and the roasting time is 3-8 hours.
8. A CO catalyst, characterized in that The CO catalyst is prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the CO catalyst according to claim 8 in catalytic oxidation of carbon monoxide.
10. The use according to claim 9, characterized in that The carbon monoxide exists in gaseous substances, the concentration of the carbon monoxide is 3000-8000 ppm, and the operating temperature of the carbon monoxide catalyst is 230-280°C.