Rod-shaped cerium-copper bimetallic Fenton-like water treatment catalyst as well as preparation method and application thereof

Through the preparation of rod-shaped cerium copper bimetal Fenton water treatment catalyst, the problems of limited pH range and high energy consumption in the prior art are solved, and the effect of efficient removal of organic pollutants within a wide pH range is achieved, and the effect of reducing the Sewage wastewater treatment cost.

CN119034755APending Publication Date: 2024-11-29GUANGZHOU UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411151703.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing advanced oxidation technology has problems such as limited pH range, high energy consumption, high cost and by-product production when removing organic pollutants in water, making it difficult to efficiently remove organic pollutants within a wide pH range.

Method used

Rod-shaped cerium copper bimetal Fenton water treatment catalyst is prepared by ultrasonic dispersion, hydrothermal reaction and multiple washing and drying to form a solid catalyst that can activate persulfate at room temperature and adapt to different pH conditions and complex environments.

Benefits of technology

It has achieved efficient removal of a variety of organic pollutants at room temperature, with long life and stability, easy recycling and recycling, reduced wastewater treatment costs, and adapted to different pH and anion environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034755A_ABST
    Figure CN119034755A_ABST
Patent Text Reader

Abstract

The invention relates to a rod-like cerium-copper bimetallic Fenton-like water treatment catalyst and a preparation method and application thereof.The preparation method of the catalyst comprises the following steps that S1, cerium nitrate and copper nitrate are dissolved in a nitric acid solution, ultrasonic dispersion is conducted till the solution is clear, and a solution A is formed; dissolving sodium hydroxide in deionized water, and uniformly stirring to form a solution B; s2, under the condition of continuous stirring, adding the solution B into the solution A, and heating and stirring to obtain a suspension C; s3, performing hydrothermal reaction on the suspension C to obtain a hydrothermal product D; and washing and drying the hydrothermal product D, grinding, soaking with deionized water, centrifuging, and drying again to obtain the catalyst CuxCeyO. The catalyst provided by the invention can efficiently remove different types of new pollutants, and can adapt to different pH conditions and complex anionic environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of sewage treatment, and in particular to a rod-shaped cerium-copper bimetallic Fenton water treatment catalyst and a preparation method and application thereof. Background Art

[0002] Water is the source of life and is related to the harmonious coexistence of man and nature.

[0003] At present, the most effective and widely used technology for removing ECs is the advanced oxidation process (AOPs) represented by the generation of reactive oxygen species (ROS) to remove organic pollutants in water. Compared with the Fenton oxidation technology that has high pH range requirements, low selectivity, easy to produce iron mud, high treatment cost, and other traditional advanced oxidation technologies that require external energy (electricity, UV, O3, etc.), the multiphase persulfate activation (PMS activation) advanced oxidation technology has attracted the attention of the academic community due to its easy availability of raw materials, significant degradation effect, and wide pH reaction range. Therefore, it is necessary to develop a water treatment technology that can activate PMS, adapt to a wide pH range, and remove organic pollutants with high efficiency and low energy consumption. Summary of the invention

[0004] In view of the problems existing in the prior art, the purpose of the present invention is to provide a rod-shaped cerium-copper bimetallic Fenton water treatment catalyst and a preparation method and application thereof.

[0005] The purpose of the present invention is achieved by the following technical solutions:

[0006] In a first aspect, the present invention provides a method for preparing a rod-shaped cerium-copper bimetallic Fenton water treatment catalyst, comprising the following steps:

[0007] S1. Dissolve cerium nitrate and copper nitrate in nitric acid solution, and disperse by ultrasonic until clear to form solution A; dissolve sodium hydroxide in deionized water, and stir evenly to form solution B;

[0008] S2. Add solution B to solution A under continuous stirring, heat and stir to obtain suspension C;

[0009] S3, subjecting the suspension C to a hydrothermal reaction to obtain a hydrothermal product D; washing and drying the hydrothermal product D, grinding it, soaking it in deionized water, centrifuging it, and drying it again to obtain a catalyst Cu x Ce y O.

[0010] Preferably, in S1, the molar ratio of cerium nitrate to copper nitrate is 2-7:1-6, more preferably 4-6:2-5.

[0011] Preferably, in S1, the molar volume ratio of cerium nitrate to nitric acid solution is (2-7) mol: (10-35) L, more preferably 5 mol: 20 L, and the concentration of nitric acid solution is 4-7 mol / L.

[0012] Preferably, in S1, the molar ratio of sodium hydroxide to cerium nitrate is 1:125, and the molar volume ratio of sodium hydroxide to deionized water is (0.5-0.625) mol:100 ml.

[0013] Preferably, in S2, the stirring temperature is 30-50°C, and the stirring time is 20-120 min.

[0014] Preferably, in S3, the hydrothermal temperature is 100-120° C., and the hydrothermal time is 20-30 h.

[0015] Preferably, in S3, washing is performed alternately with deionized water and anhydrous ethanol, and the number of washing times is 3-10 times.

[0016] Preferably, in S3, the drying temperature is 60-100° C., and the drying time is 6-12 h.

[0017] Preferably, in S3, the powder is ground to pass through a 50-100 mesh sieve; the deionized water soaking time is 24-36 hours; and the centrifugal speed is 8000-10000 rpm.

[0018] In a second aspect, the present invention provides a rod-shaped cerium-copper bimetallic Fenton water treatment catalyst prepared by the above-mentioned preparation method.

[0019] In a third aspect, the present invention provides a rod-shaped cerium-copper bimetallic Fenton water treatment catalyst for use in treating organic pollutants in sewage and wastewater.

[0020] Preferably, the organic pollutants include rhodamine B (RhB), methylene blue (MB), methyl orange (AO7), bisphenol A (BPA), ciprofloxacin (CIP), diphenhydramine (DP), and phenytoin (PHT).

[0021] Preferably, the concentration of the organic pollutants is ≥10 ppm, and the amount of the catalyst used in treating the organic pollutants in water is 0.6-1.4 g / L; the amount of persulfate (PMS) used is 2-8 mmol / L.

[0022] The beneficial effects of the present invention are:

[0023] 1. The catalyst of the present invention can activate persulfate (PMS) at normal temperature and pressure, utilize the energy of new pollutants in wastewater, and continuously treat new pollutants. During the treatment process, it can adapt to different pH conditions and complex anion environments.

[0024] 2. The catalyst of the present invention can efficiently remove different types of new pollutants and can adapt to different pH conditions and complex anion environments.

[0025] 3. The catalyst of the present invention has a long service life and stability, and it is a solid catalyst, which is easy to separate from water, convenient for recycling and recycling, and reduces the cost of sewage and wastewater treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The present invention is further described using the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the present invention. A person skilled in the art can obtain other drawings based on the following drawings without creative work.

[0027] Figure 1 This is a scanning electron microscope image of the catalyst prepared in Example 1;

[0028] Figure 2 Degradation curves of the catalyst prepared in Example 1 for pollutants PHT, RhB, AO7, BPA, and DP;

[0029] Figure 3 The degradation curve of the catalyst prepared in Example 1 to CIP at different pH values;

[0030] Figure 4 This is the degradation curve of the catalyst prepared in Example 1 to CIP under different anions. DETAILED DESCRIPTION

[0031] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.

[0032] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.

[0033] The present invention will be further described below in conjunction with the following examples.

[0034] Example 1

[0035] A rod-shaped cerium-copper bimetallic Fenton water treatment catalyst comprises the following steps:

[0036] S1: Dissolve cerium nitrate and copper nitrate (in a ratio of 5:4 mmol) in 10 mL of nitric acid (in a concentration of 4 mol / L) and disperse by ultrasonic until clear to form solution A;

[0037] S2: Dissolve 0.625 mol of sodium hydroxide in 100 ml of deionized water and stir for 20 min to form solution B;

[0038] S3: under continuous stirring, solution B was added to solution A, and after stirring at 30°C for 30 min, suspension C was obtained;

[0039] S4: subjecting the suspension C to a hydrothermal reaction at a temperature of 120°C for 24 hours, and filtering to obtain a hydrothermal product D;

[0040] S5: The hydrothermal product D was washed alternately with deionized water and anhydrous ethanol for 3 times, dried at 60°C for 10 h, ground until it could pass through an 80-mesh sieve, and then soaked in deionized water for 24 h, centrifuged (at a speed of 8000 rpm) and dried to obtain the catalyst Cu x Ce y O, its scanning electron microscope image is as follows Figure 1 shown.

[0041] Example 2

[0042] A rod-shaped cerium-copper bimetallic Fenton water treatment catalyst comprises the following steps:

[0043] S1: Dissolve cerium nitrate and copper nitrate (dosage ratio of 4:3 mmol) in 10 mL of nitric acid solution (concentration of 6 mol / L), and disperse by ultrasonic until clear to form solution A;

[0044] S2: Dissolve 0.5 mol sodium hydroxide in 100 ml deionized water and stir for 20 min to form solution B;

[0045] S3: Under continuous stirring, solution B was added to solution A, and after stirring at 35°C for 40 min, suspension C was obtained;

[0046] S4: subjecting the suspension C to a hydrothermal reaction at a temperature of 110° C. for 36 h to obtain a hydrothermal product D;

[0047] S5: The hydrothermal product D was washed alternately with deionized water and anhydrous ethanol for 3 times, dried at 80°C for 10 hours, and ground until it could pass through a 100-mesh sieve. Then, it was soaked in deionized water for 24 hours, centrifuged (at a speed of 10,000 rpm) and dried to obtain the catalyst Cu x Ce y O.

[0048] Test Example 1

[0049] The rod-shaped cerium-copper bimetallic Fenton water treatment catalyst prepared in Example 1 was used to remove different new pollutants in water; the details are as follows:

[0050] Take 0.025g of the catalyst (Cu x Ce y O) and 1mM PMS were added to 50mL, 10ppm solutions of different pollutants, kept at a constant temperature of 35°C, stirred continuously, and samples were taken at certain time intervals to detect changes in pollutant concentrations; the results are shown in Figure 2 shown.

[0051] Figure 2 The results showed that: within 5 minutes, the degradation effect on RhB reached 90%; the degradation effect on AO7 reached 100%; the degradation effect on BPA and PHT reached about 80%; the degradation effect on DP reached about 70%.

[0052] Test Example 2

[0053] The rod-shaped cerium-copper bimetallic Fenton water treatment catalyst prepared in Example 1 was used to remove the new pollutant CIP in water at different pH values; the details are as follows:

[0054] Take 0.025g of the catalyst (Cu x Ce y O) and 1mM PMS were added to 50mL, 10ppm new pollutant CIP solution, and the pH value of the pollutant solution was adjusted to 3, 5, 7, 9, and 11 respectively. The temperature was kept at 35°C, and stirring was continued. Sampling was performed at certain time intervals to detect the concentration changes of the pollutants. The results are shown in Figure 3 shown.

[0055] Figure 3 The results showed that within 5 min, the catalyst (Cu x Ce y O) The degradation effect of CIP in the environment of pH=5, 7, 9, and 11 basically reached 100%; the degradation effect of CIP in the environment of pH=3 reached about 90%.

[0056] Test Example 3

[0057] The rod-shaped cerium-copper bimetallic Fenton water treatment catalyst prepared in Example 1 was used to remove the new pollutant CIP in water under the interference of anions; the details are as follows:

[0058] Take 0.025g of the catalyst (Cu x Ce y O) and 1mM PMS were added to 50mL, 10ppm new pollutant CIP solution, and 1mM Na2HPO4, Na2SO4, NaNO3, NaCl, NaHCO3 were added respectively. The temperature was kept at 35℃, stirring was continued, and samples were taken at certain time intervals to detect the concentration changes of pollutants. The results are as follows Figure 4 shown.

[0059] Figure 4 The results showed that within 5 min, the catalyst (Cu x Ce y O) was not affected by anions and the degradation effect of CIP was basically 100% within 2 minutes.

[0060] In summary, it can be seen that the rod-shaped cerium-copper bimetallic Fenton water treatment catalyst (Cu x Ce y O) has a good degradation effect on various organic pollutants in water including RhB, MB, AO7, BPA, CIP, DP, and PHT, especially for the degradation of CIP, which can be basically completely degraded. In addition, the catalyst (Cu x Ce y O) can degrade CIP almost completely without being affected by various anions.

[0061] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.

[0062] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing a rod-shaped cerium-copper bimetallic Fenton water treatment catalyst, characterized in that: The following steps are involved: S1, dissolving cerium nitrate and copper nitrate in a nitric acid solution, and ultrasonically dispersing until clear to form a solution A; Dissolve sodium hydroxide in deionized water and stir well to form solution B; S2. Add solution B to solution A under continuous stirring, heat and stir to obtain suspension C; S3, subjecting the suspension C to a hydrothermal reaction to obtain a hydrothermal product D; washing and drying the hydrothermal product D, grinding it, soaking it in deionized water, centrifuging it, and drying it again to obtain a catalyst Cu x Ce y O.

2. The method for preparing a rod-shaped cerium-copper bimetallic Fenton water treatment catalyst according to claim 1, characterized in that: In the S1, the molar ratio of cerium nitrate to copper nitrate is 2-7:1-6, the molar volume ratio of cerium nitrate to nitric acid solution is (2-7) mol:(10-35) L, and the concentration of nitric acid solution is 4-7 mol / L.

3. The method for preparing a rod-shaped cerium-copper bimetallic Fenton water treatment catalyst according to claim 1, characterized in that: In the S1, the molar ratio of sodium hydroxide to cerium nitrate is 1:125, and the molar volume ratio of sodium hydroxide to deionized water is (0.5-0.625) mol:100 ml.

4. The method for preparing a rod-shaped cerium-copper bimetallic Fenton water treatment catalyst according to claim 1, characterized in that: In S2, the stirring temperature is 30-50°C, and the stirring time is 20-120 min.

5. The method for preparing a rod-shaped cerium-copper bimetallic Fenton water treatment catalyst according to claim 1, characterized in that: In S3, the hydrothermal temperature is 100-120° C., and the hydrothermal time is 20-30 hours; washing is performed alternately with deionized water and anhydrous ethanol, and the number of washing times is 3-10 times; the drying temperature is 60-100° C., and the drying time is 6-12 hours.

6. The method for preparing a rod-shaped cerium-copper bimetallic Fenton water treatment catalyst according to claim 1, characterized in that: In the S3, the powder is ground to pass through a 50-100 mesh sieve; the deionized water soaking time is 24-36 hours; and the centrifugal speed is 8000-10000 rpm.

7. A rod-shaped cerium-copper bimetallic Fenton water treatment catalyst, characterized in that: The preparation method according to claim 1 is used for preparation.

8. Use of the rod-shaped cerium-copper bimetallic Fenton water treatment catalyst according to claim 7 in treating organic pollutants in sewage and wastewater.

9. The use of a rod-shaped cerium-copper bimetallic Fenton water treatment catalyst in treating organic pollutants in sewage and wastewater according to claim 8, characterized in that: The organic pollutants include at least one of rhodamine B, methylene blue, methyl orange, bisphenol A, ciprofloxacin, diphenhydramine and phenytoin.

10. The use of a rod-shaped cerium-copper bimetallic Fenton water treatment catalyst in treating organic pollutants in sewage and wastewater according to claim 8, characterized in that: The concentration of the organic pollutants is ≥10 ppm, and the amount of the catalyst used in treating the organic pollutants in water is 0.6-1.4 g / L; the amount of the persulfate used is 2-8 mmol / L.