Type-II heterojunction ZnOT / ZnIn2S4-X composite catalyst for producing hydrogen through photocatalytic decomposition of water and preparation method of type-II heterojunction ZnOT / ZnIn2S4-X composite catalyst

By designing a type II heterojunction ZnOT/ZnIn2S4-X composite catalyst in a photocatalyst, using MOF-derived oxides to form a composite structure with ZnIn2S4 two-dimensional material, the problems of insufficient stability and catalytic performance of existing photocatalysts are solved, and the problem of insufficient stability and catalytic performance of existing photocatalysts is achieved. Efficient and reusable hydrogen generation is achieved, which significantly improves catalytic performance and production volume.

CN119034762APending Publication Date: 2024-11-29ANHUI UNIVERSITY OF TECHNOLOGY

Patent Information

Application Number
CN202411235073.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing photocatalysts have problems with insufficient stability and catalytic performance in the process of water decomposing hydrogen. In particular, the poor conductivity of MOF materials limits their application, and the application effect of traditional semiconductor materials in composite catalysts is limited.

Method used

Design a type II heterojunction ZnOT/ZnIn2S4-X composite catalyst to form a composite structure through oxides derived from metal organic framework material MOF and ZnIn2S4 two-dimensional material, and prepare it by gentle hydrothermal synthesis method to increase specific surface area and reaction Active sites to improve photocatalytic performance.

Benefits of technology

It achieves efficient decomposition of water to generate hydrogen, improves photocatalytic performance, is cheap, and the catalyst can be reused. The hydrogen evolution performance is retained by 96.9% after three cycles, which significantly improves the amount of hydrogen generation, exceeding the performance of ZnO and ZnIn2S4 alone.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034762A_ABST
    Figure CN119034762A_ABST
Patent Text Reader

Abstract

The invention discloses an II-type heterojunction ZnO / ZnIn2S4-X composite catalyst for producing hydrogen through photocatalytic decomposition of water and a preparation method of the II-type heterojunction ZnO / ZnIn2S4-X composite catalyst, and belongs to the technical field of photocatalytic material synthesis. The II-type heterojunction composite photocatalyst is prepared by growing a ZnIn2S4 nanosheet on the surface of the MOF-derived ZnOT. The preparation method comprises the following steps: firstly, preparing a ZIF-8 precursor, and then calcining in air at different temperatures to obtain ZnOT; the preparation method comprises the following steps: dispersing ZnOT in an aqueous solution containing anhydrous zinc chloride, indium trichloride tetrahydrate and thioacetamide in different proportions, adding glycerol, and carrying out an oil bath heating reaction to obtain composite catalysts in different proportions. The II-type heterojunction ZnO / ZnIn2S4-X composite catalyst for photocatalytic decomposition of water to generate hydrogen has good stability and catalytic performance, and a large amount of hydrogen can be generated in a short time by combining visible light to construct a photocatalytic hydrogen evolution system. Water can be efficiently decomposed to generate hydrogen, and the hydrogen can be recycled. The preparation method is simple, mild in reaction condition, economical, efficient and environment-friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a type II heterojunction ZnO photocatalytic decomposition of water to generate hydrogen. T / ZnIn 2 S 4 -X composite catalyst and preparation method, specifically suitable for photocatalytic water decomposition and efficient hydrogen evolution, belonging to the field of composite photocatalyst preparation and application technology. Background Art

[0002] With the rapid development of global industrial technology, fossil energy such as coal, oil and other non-renewable energy sources are becoming increasingly depleted. At the same time, the pollution caused by the combustion of fossil energy is also endangering the environment and human health. However, energy demand is essential for people's daily production and life, which prompts people to look for alternative renewable clean energy to alleviate the current energy pressure and environmental pollution problems. Hydrogen energy (H 2 ) As a safe, effective and sustainable energy source, it is an ideal candidate for solving the energy crisis and replacing fossil fuels. At present, a variety of technologies for producing hydrogen energy have been developed, such as electrocatalytic hydrogen production, biomass conversion hydrogen production, etc. Photocatalytic water decomposition of hydrogen is considered to be a green and sustainable solar energy conversion technology. Its principle is that semiconductor photocatalysts absorb solar energy to achieve electron transitions from the ground state to the excited state and generate sufficient energy conduction band electrons and valence band holes to meet the thermodynamic requirements of water decomposition to produce hydrogen. This technology has attracted widespread attention due to its environmental friendliness, simple methods, and wide application. Therefore, the development of highly active photocatalysts is the key to the development of this technology.

[0003] MOF materials have shown a wide range of application potentials in many fields such as gas adsorption, storage, separation and catalysis due to their high specific surface area, adjustable pore size and multifunctional properties. Especially in the field of photocatalysis, the inorganic metal center of MOF can act as an active site to achieve the generation and transfer of photogenerated charges, while the organic ligand can adjust the light absorption characteristics and charge separation efficiency. However, MOF materials have poor electrical conductivity, which limits their application in photocatalytic hydrogen production.

[0004] In recent years, MOF-derived transition metal oxides have been widely studied in the field of photocatalysis because they retain some of the advantages of MOF and have stable chemical properties. Among them, semiconductor ZnO is non-toxic and has good photocatalytic and photoelectrochemical properties, and has broad application prospects. T The favorable properties of photocatalysts can be combined with other materials to prepare heterojunction catalysts, which can increase the specific surface area of ​​the material, increase the reaction active sites, and improve the performance of photocatalytic water splitting to produce hydrogen. Therefore, it is still urgent to design a composite photocatalyst with good stability and catalytic performance that can efficiently decompose water to produce hydrogen and further expand its application field. Summary of the invention

[0005] In order to solve the problems existing in the background technology, the purpose of the present invention is to provide a composite photocatalyst with good stability and catalytic performance, which can efficiently decompose water to generate hydrogen and a preparation method thereof. It can effectively photocatalytically decompose water to generate hydrogen, establish an efficient hydrogen evolution system, effectively expand the light absorption range and enhance the photocatalytic performance.

[0006] In order to achieve the above object, the technical solution of the present invention is as follows: The first technical purpose of the present invention is to provide a type II heterojunction ZnO photocatalytic water decomposition to generate hydrogen T / ZnIn 2 S 4 -X composite catalyst, which is a metal organic framework material MOF-derived oxide and ZnIn 2 S 4 The two-dimensional materials are composited to form a type II heterojunction composite catalyst material, and the composite catalyst is prepared from a zinc source compound, an indium source compound, a sulfur source compound and a metal oxide derived from a metal organic framework material MOF.

[0007] Preferably, the zinc source compound is anhydrous zinc chloride, the indium source compound is indium trichloride tetrahydrate, the sulfur source compound is thioacetamide, and the metal organic framework material MOF-derived oxide is ZnO derived from ZIF-8.

[0008] Preferably, the molar ratio of zinc atoms, indium atoms and sulfur atoms in the zinc source compound, indium source compound and sulfur source compound is 1:2:4; the mass ratio of the zinc source compound to ZnO derived from the metal organic framework material MOF is 16~22.4:1.

[0009] Preferably, the concentration of the zinc source compound is 0.118-0.165 mol / L, the concentration of the indium source compound is 0.239-0.334 mol / L, and the concentration of the sulfur source compound is 0.480-0.672 mol / L.

[0010] The second technical purpose of the present invention is to provide a type II heterojunction ZnO photocatalytic water decomposition to generate hydrogen T / ZnIn 2 S 4 -X composite catalyst preparation method, growing ZnIn on the surface of ZnO derived from metal organic framework MOF 2 S 4 Forming a type II heterojunction specifically includes the following steps: Step 1: Preparation of MOF (ZIF-8) derived ZnO 1.68 g of zinc nitrate hexahydrate and 3.70 g of 2-methylimidazole were dissolved in methanol and dispersed evenly. The two were mixed and stirred vigorously in a beaker for 24 h to obtain a milky white solution, which was then centrifuged and washed twice with methanol. The solution was dried in an oven at 60°C overnight to obtain a metal organic framework ZIF-8. 100 mg of ZIF-8 prepared in the above steps was weighed and placed in a porcelain boat. In an air atmosphere, the heating rate was 3°C / min and calcined at different temperatures for 2 hours to obtain ZnO, which was recorded as ZnO. T (T=600, 700 and 800).

[0011] Step 2: Type II Heterojunction ZnO T / ZnIn 2 S 4 Preparation of -X composite catalyst To a 250 mL round-bottom flask, 50 mg of the ZO prepared in step 1 were added. T , 800-1120 mg of anhydrous zinc chloride, 3500-4900 mg of indium trichloride tetrahydrate, 1800-2520 mg of thioacetamide, and finally 45 mL of ultrapure water with a pH of 2.5 and 5 mL of glycerol were added to the reactor. The mixture was mixed and dispersed evenly by ultrasonication for 10 min. The oil bath was heated to 80 °C and heated for 2 h to obtain type II heterojunction ZnO. T / ZnIn 2 S 4 -X composite catalyst powder.

[0012] Step 3: Wash and dry The type II heterojunction ZnO prepared in step 2 T / ZnIn 2 S 4 The -X composite catalyst powder is washed with anhydrous ethanol for multiple times, and then the powder sample is dried naturally to obtain the type II heterojunction ZnO T / ZnIn 2 S 4 -X composite catalyst.

[0013] Preferably, the calcination temperature of the ZIF-8 precursor in step 1 is 600-800 °C.

[0014] Preferably, in step 2, the mass ratio of the ZnO derived from the metal organic framework material MOF to the ultrapure water with a pH value of 2.5 is 0.9:1.

[0015] Another object of the present invention is to provide a type II heterojunction ZnO T / ZnIn 2 S 4Application of -X composite catalyst in photocatalytic decomposition of water to generate hydrogen.

[0016] Compared with the existing detection technology, the beneficial effects of the present invention are embodied in: 1. Type II heterojunction ZnO for photocatalytic decomposition of water to generate hydrogen T / ZnIn 2 S 4 ZnO in -X composite catalyst T It is a metal oxide derived from MOF, which retains the advantages of MOF such as complex nanostructure, large specific surface area, good stability and high conductivity. The preparation method adopts a mild and simple hydrothermal synthesis method. Compared with the traditional photocatalytic process, this composite photocatalyst retains the advantages of MOF, and pure ZnIn 2 S 4 The bulk structure is a stack of sheets, but the presence of ZnO in the composite photocatalyst makes ZnIn 2 S 4 The dispersion of the nanosheets is more uniform, which effectively increases the specific surface area of ​​the material and increases the reactive sites, which is beneficial to the improvement of the photocatalytic hydrogen evolution activity; the composite photocatalyst has low cost, is controllable and easy to operate, and can efficiently generate hydrogen. 700 / ZnIn 2 S 4 -2 composite catalyst photocatalytic water decomposition can produce up to 2.47mmol g hydrogen per hour -1 , are ZnO and ZnIn 2 S 4 990 and 64 times of hydrogen evolution performance.

[0017] 2. Type II heterojunction ZnO for photocatalytic decomposition of water to generate hydrogen T / ZnIn 2 S 4 -X composite catalyst can be reused. After the first cycle, about 0.3 mL of triethanolamine was added to the photocatalytic system to replenish the loss of sacrificial reagents in the photocatalytic process, and then the system was vacuumed for 30 minutes to remove dissolved oxygen and other gases. The hydrogen evolution performance was observed again under visible light. After three cycles of use, the hydrogen evolution performance retained 96.9% of the first time.

[0018] 3. Type II heterojunction ZnO for photocatalytic decomposition of water to generate hydrogen T / ZnIn 2 S 4 Preparation method of -X composite catalyst: using ultrapure water with pH=2.5 as solvent to generate ZnIn on the surface of ZnO derived from metal organic framework material MOF 2 S 4Nanosheets, the two form a type II heterojunction. The preparation method is mild and simple, low cost, controllable and easy to operate, and the photocatalyst has strong stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The different multiples of ZnIn in the present invention 2 S 4 Type II heterojunction ZnO T / ZnIn 2 S 4 -X-ray diffraction pattern of the composite catalyst; Figure 2 Pure ZnIn 2 S 4 Scanning electron microscopy of photocatalysts; Figure 3 The type II heterojunction ZnO prepared in Example 3 of the present invention T / ZnIn 2 S 4 -Scanning electron microscopy of X composite catalyst; Figure 4 The type II heterojunction ZnO prepared in Example 3 of the present invention T / ZnIn 2 S 4 -X composite catalyst hydrogen generation rate diagram; Figure 5 The type II heterojunction ZnO prepared in Example 3 of the present invention T / ZnIn 2 S 4 -Schematic diagram of hydrogen evolution cycle performance of X composite catalyst; Figure 6 The type II heterojunction ZnO prepared in Example 3 of the present invention 700 / ZnIn 2 S 4 -2 control group ZnO 600 / ZnIn 2 S 4 and ZnO 800 / ZnIn 2 S 4 Graph of hydrogen evolution rate over composite catalyst. DETAILED DESCRIPTION

[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Embodiment 1 Step 1: Preparation of MOF (ZIF-8) derived ZnO 1.68 g of zinc nitrate hexahydrate and 3.70 g of 2-methylimidazole were dissolved in methanol and dispersed evenly. The two were mixed and stirred vigorously in a beaker for 24 h to obtain a milky white solution, which was then centrifuged and washed twice with methanol. The solution was dried in an oven at 60°C overnight to obtain a metal organic framework ZIF-8. 100 mg of the ZIF-8 prepared in the above steps was weighed and placed in a porcelain boat. In an air atmosphere, the temperature was increased at a rate of 3°C / min and calcined at 700°C for 2 hours to obtain ZnO, which was recorded as ZnO. 700 .

[0022] Step 2: Type II Heterojunction ZnO T / ZnIn 2 S 4 Preparation of -X composite catalyst Take 50 mg of ZnO derived from ZIF-8 calcined at 700 °C prepared in step 1 700 , 800 mg of anhydrous zinc chloride, 3500 mg of indium trichloride tetrahydrate and 1800 mg of thioacetamide were dispersed in 45 mL of ultrapure water with a pH of 2.5 and 5 mL of glycerol mixed solution and stirred evenly. The mixed solution was placed in a 250 mL round-bottom flask and the reaction temperature was set to 80 o C, the reaction was continued for 2 h to obtain type II heterojunction ZnO T / ZnIn 2 S 4 -X composite catalyst powder.

[0023] Step 3: Wash and dry The powder sample prepared in step 2 is washed with anhydrous ethanol for multiple times, and then the powder sample is dried naturally to obtain the type II heterojunction ZnO T / ZnIn 2 S 4 -X composite catalyst.

[0024] Embodiment 2 Step 1: Preparation of MOF (ZIF-8) derived ZnO The preparation process of this step is the same as that of Example 1.

[0025] Step 2: Type II Heterojunction ZnO T / ZnIn 2 S 4 Preparation of -X composite catalyst Take 50 mg of ZnO derived from ZIF-8 calcined at 700 °C prepared in step 1700 , 960 mg of anhydrous zinc chloride, 4200 mg of indium trichloride tetrahydrate and 2160 mg of thioacetamide were dispersed in 45 mL of ultrapure water with a pH of 2.5 and 5 mL of glycerol mixed solution and stirred evenly. The mixed solution was placed in a 250 mL round-bottom flask and the reaction temperature was set to 80 o C, the reaction was continued for 2 h to obtain type II heterojunction ZnO T / ZnIn 2 S 4 -X composite catalyst.

[0026] Step 3: Wash and dry The preparation process of this step is the same as that of Example 1.

[0027] Embodiment 3 Step 1: Preparation of MOF (ZIF-8) derived ZnO The preparation process of this step is the same as that of Example 1.

[0028] Step 2: Type II Heterojunction ZnO T / ZnIn 2 S 4 Preparation of -X composite catalyst Take 50 mg of ZnO derived from ZIF-8 calcined at 700 °C prepared in step 1 700 , 1120 mg of anhydrous zinc chloride, 4900 mg of indium trichloride tetrahydrate and 2500 mg of thioacetamide were dispersed in 45 mL of ultrapure water with a pH of 2.5 and 5 mL of glycerol mixed solution and stirred evenly. The mixed solution was placed in a 250 mL round-bottom flask and the reaction temperature was set to 80 o C, the reaction was continued for 2 h to obtain type II heterojunction ZnO T / ZnIn 2 S 4 -X composite catalyst.

[0029] Step 3: Wash and dry The preparation process of this step is the same as that of Example 1.

[0030] Embodiment 4 Step 1: Preparation of MOF (ZIF-8) derived ZnO The preparation process of this step is the same as that of Example 1, except that the ZnO obtained by calcining ZIF-8 at 600°C for 2 hours is denoted as ZnO. 600 .

[0031] Step 2: Type II Heterojunction ZnO T / ZnIn 2 S4 Preparation of -X composite catalyst The preparation process of this step is the same as that of Example 2, except that the ZnO derived from ZIF-8 added is ZnO obtained by calcining at 600°C. 600 .

[0032] Step 3: Wash and dry The preparation process of this step is the same as that of Example 1.

[0033] Embodiment 5 Step 1: Preparation of MOF (ZIF-8) derived ZnO The preparation process of this step is the same as that of Example 1, except that the ZnO derived from ZIF-8 added is ZnO obtained by calcining at 800°C for 2 hours, denoted as ZnO 800 .

[0034] Step 2: Type II Heterojunction ZnO T / ZnIn 2 S 4 Preparation of -X composite catalyst The preparation process of this step is the same as that of Example 2, except that the ZnO derived from ZIF-8 added is ZnO obtained by calcining at 800°C. 800 .

[0035] Step 3: Wash and dry The preparation process of this step is the same as that of Example 1.

[0036] Hydrogen evolution performance test Test Examples 1 to 5 prepared type II heterojunction ZnO T / ZnIn 2 S 4 -X composite catalyst and using only ZnO and ZnIn 2 S 4 As the catalysts of comparative examples 1 and 2, the performance of photocatalytic water decomposition to hydrogen under the same time and light intensity, the test results are shown in the table below.

[0037] Hydrogen evolution performance test results project Embodiment 1 Embodiment 2 Embodiment 3 Embodiment 4 Embodiment 5 Comparative Example 1 Comparative Example 2 <![CDATA[Hydrogen production amount of photocatalytic water splitting, mmol g -1 / h]]> 1.54 2.47 1.56 1.19 1.99 0.0025 0.0383 From the above performance test results of photocatalytic water decomposition and hydrogen separation, it can be seen that the type II heterojunction ZnO 700 / ZnIn 2 S 4 -2 composite catalyst photocatalytic water decomposition can produce up to 2.47mmol g hydrogen per hour -1 ; can efficiently generate hydrogen, ZnO (0.0025 mmol g -1 h -1 ) and ZnIn2 S 4 (0.0383 mmol g -1 h -1 ) has a hydrogen evolution performance of 990 and 64 times. The present invention has no type II heterojunction ZnO T / ZnIn 2 S 4 -X composite catalyst can be reused, and after three cycles of use, the hydrogen evolution performance is retained to 96.9% of the first time. Figure 5 . It is proved that the type II heterojunction ZnO T / ZnIn 2 S 4 -X composite catalyst can not only efficiently decompose water to generate hydrogen, but also can be recycled and reused. The preparation method of the invention is simple, the reaction conditions are mild, and it is economical, efficient and environmentally friendly.

[0038] What is described above is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A Type II Heterojunction ZnO Photocatalytic Water Decomposition to Generate Hydrogen T / ZnIn2S4-X composite catalyst, characterized by: It is a type II heterojunction composite catalyst formed by a composite of an oxide derived from a metal organic framework material MOF and a ZnIn2S4 two-dimensional material. The composite catalyst is prepared from a zinc source compound, an indium source compound, a sulfur source compound and a metal oxide derived from a metal organic framework material MOF.

2. A type II heterojunction ZnO for photocatalytically decomposing water to generate hydrogen according to claim 1 T / ZnIn2S4-X composite catalyst, characterized by: The zinc source compound is anhydrous zinc chloride, the indium source compound is indium trichloride tetrahydrate, the sulfur source compound is thioacetamide, and the oxide derived from the metal organic framework material MOF is ZnO derived from ZIF-8.

3. A type II heterojunction ZnO for photocatalytically decomposing water to generate hydrogen according to claim 1 T / ZnIn2S4-X composite catalyst, characterized by: The molar ratio of zinc atoms, indium atoms and sulfur atoms in the zinc source compound, indium source compound and sulfur source compound is 1:2:4; the mass ratio of the zinc source compound to ZnO derived from the metal organic framework material MOF is 16-22.4:

1.

4. A type II heterojunction ZnO for photocatalytically decomposing water to generate hydrogen according to claim 1 T / ZnIn2S4-X composite catalyst, characterized by: The concentration of the zinc source compound is 0.118-0.165 mol / L, the concentration of the indium source compound is 0.239-0.334 mol / L, and the concentration of the sulfur source compound is 0.480-0.672 mol / L.

5. A method for preparing the type II heterojunction ZnO for photocatalytic water decomposition to generate hydrogen as claimed in claim 1 T / ZnIn2S4-X composite catalyst method, characterized in that: Type II heterojunction ZnO prepared by growing ZnIn2S4 on the surface of MOF-derived ZnO T / ZnIn2S4-X composite catalyst.

6. A type II heterojunction ZnO for photocatalytically decomposing water to generate hydrogen according to claim 5 T / A method for preparing a ZnIn2S4-X composite catalyst, characterized in that The steps include: Step 1: Preparation of ZIF-8-derived ZnO 1.68 g zinc nitrate hexahydrate and 3.70 g 2-methylimidazole were dissolved in methanol respectively, and after being evenly dispersed, the two were mixed and vigorously stirred in a beaker for 24 h to obtain a milky white solution; then the solution was centrifuged and washed twice with methanol, and dried in an oven at 60 °C overnight to obtain a metal organic framework MOF material ZIF-8; 100 mg of the ZIF-8 prepared in the above steps was weighed and put into a porcelain boat, and in an air atmosphere, the heating rate was 3 °C / min, and calcined at different temperatures for 2 hours to obtain ZnO, which was recorded as ZnO T ; Step 2: Type II Heterojunction ZnO T Preparation of / ZnIn2S4-X composite catalyst Into a 250 mL round-bottom flask, 50 mg of the ZnO prepared in step 1 was added. T , 800-1120 mg of anhydrous zinc chloride, 3500-4900 mg of indium trichloride tetrahydrate, 1800-2520 mg of thioacetamide, and finally 45 mL of ultrapure water with a pH of 2.5 and 5 mL of glycerol were added to the reactor. The mixture was mixed and dispersed evenly by ultrasonication for 10 min, and then the oil bath was heated to 80 °C. After heating for 2 h, the powdered type II heterojunction ZnO was obtained by reaction. T / ZnIn2S4-X composite catalyst.

7. A type II heterojunction ZnO for photocatalytically decomposing water to generate hydrogen according to claim 6 T / A method for preparing a ZnIn2S4-X composite catalyst, characterized in that: The calcination temperature of the ZIF-8 precursor in step 1 is 600-800 °C.

8. A type II heterojunction ZnO for photocatalytically decomposing water to generate hydrogen according to claim 6 T / A method for preparing a ZnIn2S4-X composite catalyst, characterized in that: The mass ratio of ZnO to ultrapure water with a pH value of 2.5 in step 2 is 0.9:

1.

9. A type II heterojunction ZnO for photocatalytically decomposing water to generate hydrogen according to claim 6 T / A method for preparing a ZnIn2S4-X composite catalyst, characterized in that: The method further comprises: preparing the type II heterojunction ZnO prepared in step 2 T The / ZnIn2S4-X composite catalyst powder was washed with anhydrous ethanol for multiple times and then dried naturally.

10. A type II heterojunction ZnO as claimed in any one of claims 1 to 9 T Application of / ZnIn2S4-X composite catalyst in photocatalytic water decomposition to generate hydrogen.

Citation Information

Patent Citations

  • Method for preparing ZnO crystal based on ZIF-8

    CN111185150A

  • Photocatalyst as well as preparation method and application thereof

    CN114588888A

Cited By

  • Three-phase composite photocatalyst as well as preparation method and application thereof