Preparation method and application of denitration catalyst

Preparation of copper manganese oxide catalysts by molten salt method solves the high cost and environmental pollution problems of traditional vanadium tungsten titanium catalysts in flue gas denitrogen, and achieves efficient and stable flue gas denitrogenation effect, reducing production costs and reducing three wastes emission.

CN119034769APending Publication Date: 2024-11-29WUHAN KELIN FINE CHEM
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411336795.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

When traditional vanadium tungsten titanium catalysts are used in industry for flue gas denitrification, there are problems such as high cost, narrow applicable temperature, harsh usage conditions, easy to poison, short life and three waste emissions. The existing synthesis methods are difficult to control the reaction components, resulting in the catalyst. Unstable performance.

Method used

The denitrition catalyst with copper-manganese oxide as the main active component is prepared by molten salt method. Through grinding pretreatment, melt oxidation treatment and catalyst molding treatment, a copper-manganese oxide catalyst with high catalytic activity is formed, which is used for selective catalytic reduction technology. middle.

Benefits of technology

It achieves low-cost and efficient flue gas denitrification, reduces waste emissions, improves the stability and applicable temperature range of catalysts, reduces production costs, and meets environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a denitration catalyst, a molten salt method is adopted for preparation, and the preparation method specifically comprises the following steps: mixing and grinding a raw material metal precursor and a molten salt auxiliary agent, carrying out calcination melting and oxidation treatment in a crucible to obtain a catalytic active component, and finally adding a carrier and the auxiliary agent for molding to prepare the SCR denitration catalyst, the prepared catalyst has excellent denitration performance under industrial conditions. The preparation method is simple and convenient, the equipment investment is small, no three wastes are discharged, and the prepared catalyst is excellent in effect and stable in structure. The method not only can produce the denitration catalyst with extremely high catalytic activity at low cost, but also can reduce the emission of three wastes in the preparation and use processes of the traditional vanadium-tungsten-titanium denitration catalyst and reduce the harm to the environment, and is suitable for large-scale use in industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of industrial catalysis, and in particular to a preparation method and application of a denitration catalyst. Background Art

[0002] With the rapid development of industry, the total amount of industrial flue gas has also increased greatly, among which nitrogen oxides (NO x ) seriously pollutes the atmospheric environment. Therefore, flue gas denitrification technology is in urgent need of development and application. At present, the most commonly used nitrogen oxide control technology in industry is selective catalytic reduction technology (SCR), in which the denitrification catalyst used converts harmful nitrogen oxides into harmless nitrogen through catalytic reaction for safe emission. The traditional vanadium tungsten titanium catalyst is relatively mature, but it has the problems of high cost, narrow applicable temperature, harsh use conditions, easy poisoning, short life, and the generation of three wastes during production and use, which need to be solved urgently.

[0003] Generally speaking, coprecipitation, impregnation and hydrothermal methods are commonly used methods for synthesizing denitration catalysts. For example, the preparation of a V2O5 / TiO2 low-temperature NH3-SCR catalyst and its application in denitration disclosed in patent CN201510445462, the vanadium-based catalyst prepared by the impregnation method has a good denitration effect. However, due to the different solubility of the substances and the influence of various synthesis conditions (such as solution temperature, liquid pH, aging time, drying method, etc.), the reaction between the components is difficult to control. In addition, in the industrial production process, the dissolution and leaching of soluble toxic substances is inevitable. In contrast, the molten salt method melts and crystallizes the raw materials at high temperature, and then oxidizes them to form mixed oxides, which enhances the contact of the raw materials, thereby reducing the reaction start temperature, shortening the reaction time, and eliminating the discharge of waste liquid. The molten salt method for synthesizing catalysts has the advantages of low cost, simple operation, and simple equipment. For example, in the patent CN202210907775, it is mentioned that the molten salt method can make the active components dispersed better and improve the performance of the catalyst. The patent CN201510194001 discloses a method for preparing AgCl / LiNbO3 composite photocatalyst by molten salt method, which also mentions the advantages of the molten salt method for the preparation of catalysts. Therefore, the molten salt method is a suitable method for synthesizing denitrification catalysts. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a preparation method and application of a denitration catalyst. The method can not only produce a denitration catalyst with extremely high catalytic activity at a low cost, but also reduce the discharge of three wastes during the preparation and use of traditional vanadium, tungsten and titanium denitration catalysts, thereby reducing harm to the environment.

[0005] To achieve the above object, the technical solution of the present invention is achieved as follows: A preparation method and application of a denitration catalyst, characterized in that the active component of the catalyst is mainly copper manganese oxide, and the catalyst is prepared by a molten salt method, comprising the following steps: S1. Grinding pretreatment: using transition metal salt as raw material, sodium phosphate and potassium phosphate as molten salt additives, The raw materials and additives are fully mixed according to proportion, put into a grinder and fully ground to obtain a mixture.

[0006] The purpose of this step is to evenly distribute the raw materials and additives to facilitate subsequent processing; S2. Melt oxidation treatment: the mixture obtained in S1 is placed in a crucible, and melt-crystallized at high temperature in an inert gas atmosphere, and then the mixture is oxidized in an air atmosphere, and then cooled to obtain an oxidized mixture.

[0007] The purpose of this step is to melt and crystallize the raw materials and additives at high temperature, and then evenly oxidize them into mixed metal oxides to obtain active components.

[0008] S3. Catalyst molding treatment: The oxidation mixture obtained in S2 is crushed, mixed with the catalyst carrier and the auxiliary agent in proportion, and then molded to prepare a denitration catalyst.

[0009] Preferably, the transition metal salt in step S1 is a manganese metal salt or a copper metal salt; In terms of mass percentage, manganese metal salt accounts for 50-80% of the total metal salt, and copper metal salt accounts for 20-50% of the total metal salt; The manganese metal salt is one or more of manganese acetate, manganese sulfate, and manganese carbonate; the copper metal salt is one or more of copper nitrate, basic copper carbonate, and basic copper sulfate; Preferably, the mass percentage of the transition metal salt raw material and the molten salt additive in step S1 is: the transition metal salt raw material is 80-98%, and the molten salt additive is 2-20%.

[0010] Preferably, the grinding speed in step S1 is 50-600 r / min, and the grinding time is 1-6 h.

[0011] Preferably, the inert atmosphere in step S2 is nitrogen or argon.

[0012] Preferably, the high temperature melting crystallization temperature in step S2 is 700-1000°C, the melting time is 3-6 h, and the subsequent mixture oxidation temperature is 300-600°C, and the oxidation time is 3-6 h.

[0013] Preferably, the catalyst carrier in step S3 is one or more of alumina, titanium dioxide, and silicon dioxide, and the auxiliary agent is one or more of polyethylene glycol and sesbania powder. In terms of the total mass percentage of the catalyst, the active component accounts for 5%-25%, the auxiliary agent accounts for 2%-5%, and the rest is the carrier.

[0014] The application of molten salt method to prepare denitrification catalyst includes the following features: Preferably, the catalyst can be used for the selective catalytic reduction flue gas denitration reaction of boiler exhaust gas, factory flue gas and automobile exhaust.

[0015] When the reaction conditions are NO x The content is 1000 ppm, the O2 content is 10%, the reducing agent is 1000 ppm ammonia, and the reaction space velocity is 20000 h -1 When the reaction temperature is 150-300 ℃, the denitrification efficiency of the catalyst can reach more than 90%.

[0016] The flue gas denitration catalyst prepared by the molten salt method of the present invention can make the flue gas meet the national emission standards under conventional flue gas conditions. According to the relevant national standards, the specific surface area of ​​the obtained catalyst is 40-350 m 2 / g, pore volume is 0.1-0.5 m 3 / g, average pore size of 10-300 nm, at a space velocity of 20000 h -1 When the raw gas is 1000 ppm NO, 10% O2, the reaction temperature is 200 °C, and 1000 ppm NH3 is added, the NO conversion rate can reach 100%.

[0017] Compared with the prior art, the molten salt method for preparing catalysts and the application provided by the present invention have the following advantages: (1) The molten salt method used in the present invention can enhance the interaction between the raw materials interface, which is conducive to the directional formation of the catalyst crystal structure, thereby constructing a denitration catalyst with controllable crystal form and shape, so that the catalyst has excellent SCR catalytic activity, good stability during the catalytic process, and can treat NO x The concentration range is wide. In practical applications, there is no need to make major modifications to the original exhaust emission system. It is in line with my country's actual national conditions, easy to promote and use, and has a high application prospect.

[0018] (2) The present invention utilizes the molten salt method to prepare the catalyst, which is green and environmentally friendly, without the discharge of three wastes. It avoids the emission of harmful substances during the preparation and use of the existing vanadium tungsten titanium denitrification catalyst, and also greatly reduces the production cost of the denitrification catalyst, which has positive significance for the protection of the ecological environment and economic development. DETAILED DESCRIPTION

[0019] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0020] The principles and features of the present invention are described below. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention. Example 1

[0021] 40 g MnSO4 and 40 Cu2(OH)2SO4 were used as raw materials, 10 g Na3PO4 and 10 g K3PO4 were used as molten salt additives. After the raw materials and additives were fully mixed, they were put into a grinder and ground at a rate of 50 r / min for 1 h to obtain a mixture of about 100 g. The obtained mixture was placed in a crucible and melted and crystallized for 3 h at 700 °C in a nitrogen atmosphere, then cooled to 300 °C, and then air was introduced to oxidize the mixture for 3 h. After cooling, an oxidized mixture was obtained, that is, about 50 g of catalytically active substances. After the obtained catalytically active substances were crushed to less than 100 mesh, 930 g alumina was added as a carrier, and 20 g sesbania powder was added as an auxiliary agent, a total of 1000 g of the mixture was formed to make denitration catalyst #1. According to the total mass percentage of the catalyst, the active component accounted for 5%, the auxiliary agent accounted for 2%, and the rest was the carrier. Example 2

[0022] 20 g Cu(NO3)2 and 78 g MnCO3 were used as raw materials, 1 g Na3PO4 and 1 g K3PO4 were used as molten salt additives. After the raw materials and additives were fully mixed, they were put into a grinder and ground at a rate of 600 r / min for 6 h to obtain a mixture of about 100 g. The obtained mixture was placed in a crucible and melted and crystallized at 1000 °C in an argon atmosphere for 6 h, then cooled to 600 °C, and then air was introduced to oxidize the mixture for 6 h. After cooling, an oxidized mixture, i.e., about 50 g of catalytically active substances, was obtained. After the obtained catalytically active substances were crushed to less than 100 mesh, 140 g titanium dioxide was added as a carrier, 5 g sesbania powder, and 5 g polyethylene glycol were added as additives, and a total of 200 g of the mixture was formed to prepare denitration catalyst #2. According to the total mass percentage of the catalyst, the active component accounted for 25%, the additive accounted for 5%, and the rest was the carrier. Example 3

[0023] 30 g Cu2(OH)2CO3 and 60 g (CH3COO)2Mn were used as raw materials, 5 g Na3PO4 and 5 g K3PO4 were used as molten salt additives. After the raw materials and additives were fully mixed, they were put into a grinder and ground at a rate of 200 r / min for 3 h to obtain a mixture of about 100 g. The obtained mixture was placed in a crucible and melted and crystallized at 700 ° C in a nitrogen atmosphere for 6 h, then cooled to 400 ° C, and then air was introduced to oxidize the mixture for 6 h. After cooling, an oxidized mixture was obtained, that is, about 50 g of catalytically active substances. After the obtained catalytically active substances were crushed to less than 100 mesh, 440 g silica was added as a carrier and 10 g polyethylene glycol as an auxiliary agent, a total of 500 g of the mixture was formed to make denitration catalyst #3. According to the total mass percentage of the catalyst, the active component accounted for 10%, the auxiliary agent accounted for 2%, and the rest was the carrier. Example 4

[0024] 45 g MnSO4, 30 g MnCO3, 10 g Cu2(OH)2CO3 were used as raw materials, 7.5 g Na3PO4, 7.5 g K3PO4 were used as molten salt additives, the raw materials and additives were fully mixed, put into a grinder and ground at a rate of 200 r / min for 6 h to obtain a mixture of about 100 g. The obtained mixture was placed in a crucible, melted and crystallized at 700 ° C in an argon atmosphere for 3 h, then cooled to 500 ° C, and then air was introduced to oxidize the mixture for 3 h. After cooling, an oxidized mixture was obtained, that is, about 60 g of catalytically active substances. After the obtained catalytically active substances were crushed to less than 100 mesh, 100 g alumina, 98 g titanium dioxide, 30 g silicon dioxide were added as carriers and 12 g sesbania powder as auxiliary agents, a total of 300 g of the mixture was formed to make denitration catalyst #4. According to the total mass percentage of the catalyst, the active component accounted for 20%, the auxiliary agent accounted for 4%, and the rest was the carrier.

[0025] The effect of denitrification catalyst can be divided into activity test and stability test.

[0026] Activity test: Tested in a fixed bed reactor at normal pressure. The catalyst was dried, crushed and sieved to 20-40 mesh. 3 mL of catalyst was added to a quartz tube with an inner diameter of 6 mm and placed in the reactor. The reaction gas composition was 1000 ppm NO x , 10% O2, 1000 ppm NH3, N2 balance, space velocity 20000 h -1 , the reaction temperatures are 150°C, 250°C, and 300°C, and the outlet gas is continuously measured by a flue gas analyzer.

[0027] The denitrification efficiency is calculated by the following formula:

[0028] Among them, NO x The concentration is the total concentration of NO+NO2.

[0029] The activity test data of the denitration catalyst prepared in the examples are shown in Table 1.

[0030] Table 1 Activity data of various catalysts at different temperatures

[0031] Stability test: Tested in a fixed bed reactor at normal pressure. The catalyst was dried, crushed and sieved to 20-40 mesh. 3 mL of catalyst was added to a quartz tube with an inner diameter of 6 mm and placed in the reactor. The reaction gas composition was 1000 ppm NO, 10% O2, 1000 ppm NH3, 100 ppm SO2, 10% H2O, N2 balance, and the space velocity was 20000 h -1 , the reaction temperature was 250 °C, the reaction time was 24 h, 72 h, and 168 h, and the outlet gas was continuously measured by a flue gas analyzer.

[0032] The denitrification efficiency is calculated by the following formula:

[0033] Among them, NO x The concentration is the total concentration of NO+NO2.

[0034] The stability data of the denitration catalyst prepared in the examples are shown in Table 2.

[0035] Table 2 Stability data of each catalyst at different time

[0036] Based on the above test results, it can be seen that the denitrification catalysts made by the molten salt method have good SCR denitrification activity and stability.

[0037] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A preparation method and application of a denitration catalyst, characterized in that: The active component of the catalyst is mainly copper manganese oxide, and the catalyst is prepared by a molten salt method, comprising the following steps: S1. Grinding pretreatment: using transition metal salt as raw material, sodium phosphate and potassium phosphate as molten salt additives, The raw materials and additives are mixed in proportion, and put into a grinder for grinding to obtain a mixture; S2, melt oxidation treatment: the mixture obtained in S1 is placed in a crucible, and high-temperature melt crystallization is performed under an inert gas atmosphere, and then the mixture is oxidized under an air atmosphere, and after cooling, an oxidized mixture is obtained, that is, an active component is obtained; S3, catalyst molding treatment: crushing the oxidation mixture obtained in S2, mixing it with the catalyst carrier and the additive in proportion, and molding it to prepare a denitration catalyst; The catalyst is used to catalyze the NH3 reduction flue gas denitration reaction, using NH3 and NO x The redox reaction converts NO x Switch to N2 for removal.

2. The preparation method according to claim 1, characterized in that: The transition metal salt in step S1 is a manganese metal salt and a copper metal salt; in terms of mass percentage, the manganese metal salt accounts for 50-80% of the total metal salts, and the copper metal salt accounts for 20-50% of the total metal salts.

3. The preparation method according to claim 2, characterized in that: The manganese metal salt is one or more of manganese acetate, manganese sulfate, and manganese carbonate, and the copper metal salt is one or more of copper nitrate, basic copper carbonate, and basic copper sulfate.

4. The preparation method according to claim 1, characterized in that: The mass percentage of the transition metal salt raw material and the molten salt additive in step S1 is: 80-98% of the transition metal salt raw material and 2-20% of the molten salt additive; the grinding speed in step S1 is 50-600 r / min, and the grinding time is 1-6 h.

5. The preparation method according to claim 1, characterized in that: The inert atmosphere in step S2 is one of nitrogen or argon; the high temperature melting crystallization temperature is 700-1000°C, the melting time is 3-6 h, and the subsequent mixture oxidation temperature in air atmosphere is 300-600°C, and the oxidation time is 3-6 h.

6. The preparation method according to claim 1, characterized in that: The catalyst carrier in step S3 is one or more of alumina, titanium dioxide, and silicon dioxide, and the auxiliary agent is one or more of polyethylene glycol and sesbania powder; based on the total mass percentage of the catalyst, the active component accounts for 5%-25%, the auxiliary agent accounts for 2%-5%, and the rest is the carrier.

7. The use according to claim 1, characterized in that: The reaction conditions of the application are NO x The content is 1000ppm, the O2 content is 10%, the reducing agent is 1000 ppm ammonia added, and the reaction space velocity is 20000 h -1 When the reaction temperature is 150-300℃, the catalyst denitrification efficiency reaches more than 90%.

Citation Information

Patent Citations

  • Method for preparing AgCl / LiNbO3 composite photo-catalyst through salt self-fusing method

    CN104815680A

  • Preparation of low-temperature NH3-SCR catalyst with slice-shaped V2O5 / TiO2 as carrier and application of catalyst in denitration

    CN105032398A

  • Catalyst suitable for wet reforming of methane, preparation method, reduction method and application method

    CN115282975A