Method for manufacturing spinning die through laser additive manufacturing technology and spinning die
Spinning molds are manufactured through laser additive technology, combining heat treatment and tempering treatment, and solving the problems of high production cost and short service life of spinning molds, achieving high hardness and wear resistance molds, and achieving multiple repairs and utilization , reducing the cost of material scrapping.
Patent Information
- Application Number
- CN202411479810.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-23
- Publication Date
- 2024-11-29
AI Technical Summary
The existing spinning mold production methods are costly, have a long production cycle, and are easy to damage and difficult to repair, resulting in a short service life.
The spinning mold is manufactured using laser additive technology, and the mold steel powder is manufactured through laser additive and heat treatment is carried out. Combined with tempering and finishing, high hardness and wear resistance molds are obtained, and multiple repairs are achieved.
It reduces the production cost and cycle of spinning molds, improves the service life and wear resistance of the molds, realizes the recycling of materials, and solves the high cost problems caused by the scrapping of raw materials.
Smart Images

Figure CN119035384A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of laser additive manufacturing, and in particular to a method for manufacturing a spinning mold using laser additive manufacturing technology and a spinning mold. Background Art
[0002] The spinning die is an important die in the spinning process of barrel-shaped parts, and is a key part to ensure processing accuracy and quality. During long-term use, the spinning die is subjected to high-intensity extrusion and wear, and the use conditions are harsh. The failure modes of the spinning die are usually axial strain, surface wear, and insufficient precision caused by extrusion deformation. Any failure can cause the spinning die to be unable to be used normally, resulting in property loss and waste.
[0003] Common spinning die materials are cold working die steel, such as Cr12MoV, 70Cr3NiMo, etc. At present, cold working die steel spinning dies have the following problems: 1. The forging and heat treatment system of this type of die steel is complex and the process control is difficult; 2. Since cold working die steel has high carbon content and poor weldability, it is very easy to produce welding cracks. In addition, the structure of this type of die steel changes after welding and cannot be welded again, so secondary repair is not possible; 3. Such materials have high costs, long manufacturing cycles, and are difficult to reuse.
[0004] Laser additive manufacturing (LAM) technology is an additive manufacturing technology that uses laser as an energy source. Laser has the characteristics of high energy density and can realize the manufacturing of difficult-to-process metals, such as titanium alloys and high-temperature alloys used in the aerospace field. At the same time, laser additive manufacturing technology also has the advantage of not being restricted by part structure and can be used for the processing and manufacturing of complex, difficult-to-process and thin-walled parts. Summary of the invention
[0005] The technical problem to be solved by the present invention is that the existing spinning mold manufacturing method has the problems of high cost and long manufacturing cycle.
[0006] In order to solve the above problems, the present invention proposes the following technical solutions: In one aspect, the present invention provides a method for making a spinning mold using laser additive technology, comprising the following steps: S1. Performing laser additive manufacturing on the surface of the forging blank to be processed to obtain a mold precursor; S2, heat treating the mold precursor to obtain a spinning mold; The laser additive process parameters in step S1 include: a linear speed of 20 to 70 mm / s; an overlap rate of 35 to 50%; and a laser power of 3000 to 6000 W.
[0007] Furthermore, the powder used for laser additive manufacturing in step S1 is at least one of die steel and high-speed steel alloy, such as Cr12MoV alloy powder, M2 alloy powder, etc.
[0008] Furthermore, the particle size of the powder used in the laser additive manufacturing in step S1 is 15-200 μm, preferably 30-150 μm, and more preferably 50-100 μm.
[0009] Furthermore, the thickness of the laser additive in step S1 is 3 to 8 mm.
[0010] Furthermore, in step S1, the thickness of a single layer of laser additive manufacturing is 0.3-1.4 mm, which can ensure the post-processing allowance after additive manufacturing.
[0011] Furthermore, in step S2, the heat treatment process includes quenching and high-temperature tempering; wherein the quenching temperature is 950-1050°C, and the high-temperature tempering temperature is 510-520°C. Heat treatment can improve the comprehensive mechanical properties of the workpiece.
[0012] Furthermore, the heat treatment process also includes stress relief annealing, and the stress relief annealing temperature is 220-280° C. Stress relief annealing helps to improve the bonding strength between the laser additive layer material and the blank material.
[0013] Furthermore, the heat treatment process is specifically as follows: keeping the temperature at the stress relief annealing temperature for 4 to 10 hours, then keeping the temperature at the quenching temperature for 4 to 8 hours and then oil cooling, and then keeping the temperature at the high temperature tempering temperature for not less than 4 hours.
[0014] Furthermore, the quenching is performed 1 to 3 times, and the high temperature tempering is performed 1 to 3 times.
[0015] Furthermore, the material of the forging blank is alloy structural steel, such as 42CrMo alloy structural steel, 42CrMnTi alloy structural steel, etc.
[0016] Furthermore, before step S1, the forging blank to be processed is subjected to quenching and tempering treatment, and then turned to reserve a processing allowance.
[0017] Specifically, before step S1, the forging blank to be processed is further subjected to quenching and tempering treatment, and the quenched and tempered forging blank is turned to leave a finishing allowance for later heat treatment deformation and laser additive thickness.
[0018] It should be noted that, in the present invention, the quenching and tempering treatment refers to a double heat treatment method of quenching and high-temperature tempering, the purpose of which is to make the blank workpiece have good comprehensive mechanical properties. The quenching and tempering can greatly adjust the performance and material of the steel, and its strength, plasticity and toughness are all good. Technical personnel in this field can select the quenching and tempering treatment process according to the material of the forging blank, and the present invention does not limit this.
[0019] Furthermore, after step S2, the method further includes: step S3, finishing the heat-treated parts according to the requirements of the drawings to obtain a spinning mold.
[0020] Specifically, the finishing methods include turning and grinding. After finishing, the performance indicators of the sample must be tested according to the drawings and technical requirements. For example, form and position tolerances, dimensional tolerances and surface finish shall be tested according to the drawings, and non-destructive testing shall be carried out according to the technical requirements or GJB-2376A-2005, GB / T 42401-2023 and GB / T 5777-2019 U1 level.
[0021] Furthermore, all the above processing steps adopt the same reference double top processing.
[0022] On the other hand, the present invention further provides a spinning mold, which is prepared by the preparation method described in the first aspect, wherein the surface hardness of the spinning mold is above 60HRC and the depth of the hardened layer is 25 to 30 mm.
[0023] Compared with the prior art, the technical effects achieved by the present invention include: The method for manufacturing a spinning mold using laser additive technology provided by the present invention replaces cold working die steel in manufacturing the spinning mold, and can effectively reduce the problems of high cost and long manufacturing cycle in the manufacturing process of the spinning mold. The spinning mold manufactured using laser additive manufacturing has higher strength and wear resistance, and greatly improves the service life of the spinning mold. In addition, the spinning mold with surface wear can be repaired using additive powder by laser additive manufacturing to restore the mold accuracy, and the spinning mold can be repaired and utilized multiple times.
[0024] Furthermore, by utilizing the method of the present invention, mold steel and high-speed steel alloy powder are used as raw materials for additive manufacturing. After laser additive manufacturing and heat treatment processes, the hardness of the obtained spinning mold reaches above 60HRC, and the effective hardened layer depth is 25 to 30 mm, which improves the surface wear resistance and strength of the spinning mold and greatly improves the service life of the spinning mold.
[0025] Furthermore, using the method of the present invention, alloy structural steel can be used as the core material of the spinning mold. In combination with the alloy powder raw material and heat treatment process used for additive manufacturing, the core material has a high degree of compatibility with the alloy powder raw material of the additive manufacturing, has a strong bonding force, has a low material cost, and the heat treatment process is simple and controllable, thereby reducing the manufacturing cost.
[0026] The spinning mold made by the method for making a spinning mold using laser additive technology provided by the present invention not only has high surface mechanical properties, but also has excellent repairability. The spinning mold can be cyclically repaired by the laser additive method, thereby realizing material recycling and completely solving the high cost problem caused by the scrapping of raw materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying any creative work.
[0028] Figure 1 A schematic flow chart of a method for making a spinning mold using laser additive technology provided by the present invention; Figure 2 This is a metallographic photograph of the blank substrate layer and the additive layer of the spinning mold M403 Example 2 obtained by the method of the present invention, the upper half is the blank substrate layer, and the lower half is the additive layer. DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments. Obviously, the embodiments described below are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] It should be understood that when used in this specification and the appended claims, the terms "include" and "comprises" indicate the presence of described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.
[0031] It should also be understood that the terms used in this description of the embodiments of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the embodiments of the present invention. As used in the description of the embodiments of the present invention and the appended claims, unless the context clearly indicates otherwise, the singular forms of "a", "an" and "the" are intended to include plural forms.
[0032] The method of the present invention is described in detail below with reference to batch spinning mold production: Example 1: Use laser additive manufacturing to make one M403 and one M632 spinning mold: The surface hardness is required to be ≥60HRC, the thickness of the effective additive functional layer is ≥2.5mm, the overall effective hardened layer depth is 25-30mm, the surface finish is below Ra0.4, and the functional layer has no defects such as cracks, pores, poor fusion, etc. Other dimensions and shape and position tolerances meet the requirements of the drawings.
[0033] It can be understood that the effective functional layer refers to the effective thickness of laser additive manufacturing.
[0034] See also Figure 1 , the spinning mold is manufactured by using the method for manufacturing a spinning mold using laser additive technology provided by the present invention: Step 1) reprocessing the forging blank; Step 1.1) machining center positioning holes at both ends of two quenched and tempered 42CrMo forging blanks; Step 1.2) Turning is performed based on the center positioning hole processed in step 1.1). A finishing allowance of 1mm is reserved for post-heat treatment deformation in the non-additive area, and a laser additive thickness of 2.5mm + heat treatment deformation allowance of 1mm is reserved in the additive area.
[0035] Step 2) Laser additive manufacturing; The two blank parts completed in step 1) were respectively subjected to additive manufacturing in the areas to be added. The laser additive manufacturing parameters used were: line speed of 30 mm / s; overlap rate of 50%; laser power of 4000 W; single layer thickness of 1 mm, number of layers of 3, and the powder used for additive manufacturing was Cr12MoV alloy powder with a particle size of 50-80 μm.
[0036] Step 3) heat treatment; After completing step 2), the workpiece is heat treated by quenching and high-temperature tempering the entire workpiece (including the additive area and the non-additive area) at a quenching temperature of 1000°C. After keeping warm for 6 hours, it is oil-cooled and then tempered at a high temperature of 520°C for 4 hours.
[0037] Step 4) Finishing; Step 4.1) After completing step 3), turn the parts according to the M403 and M632 drawings. The non-additive areas are directly machined to the drawing size, and a 0.15mm grinding allowance is reserved for the additive areas.
[0038] Step 4.2) After completing step 4.1), the additive area is ground to achieve the dimensional tolerance and surface finish required by the drawing.
[0039] Step 5) Inspection: Carry out relevant inspection data according to the requirements of the drawing as shown in Table 1.
[0040] The workpieces manufactured by the above method are named M403 Example 1 and M632 Example 1.
[0041] Example 2 This embodiment optimizes the heat treatment process of step 3) on the basis of the processing steps of step 1, and the other operations remain unchanged. The specific heat treatment method is to perform stress relief annealing, quenching and two high-temperature tempering on the entire workpiece (including the additive area and the non-additive area) in sequence, the stress relief annealing temperature is 250℃, and the heat preservation time is 8h, the quenching temperature is 1050℃, and the heat preservation time is 6h, and then oil cooling, and then the first high-temperature tempering is performed, the high-temperature tempering temperature is 520℃, and the heat preservation time is 4h, and the second high-temperature tempering is performed, and the high-temperature tempering temperature is 520℃, and the heat preservation time is 4h.
[0042] The workpieces manufactured by the method of this embodiment are named M403 Example 2 and M632 Example 2.
[0043] Metallographic photos of M403 type 2 are shown in Figure 2 , it can be seen that the blank layer and the laser additive layer are well combined.
[0044] Table 1 Final inspection record
[0045] Among them, fluorescence detection is carried out according to GJB-2376A-2005 and GB / T 42401-2023; Ultrasonic testing is carried out according to GB / T 5777-2019 U1 level.
[0046] The effective hardened layer depth of the above spinning die is tested according to GB / T 5617-2005.
[0047] According to the test results, the dimensional tolerance, form and position tolerance, surface finish, hardness and other test items meet the requirements of the drawings. There are no cracks, pores, unfused surfaces or other defects that affect the quality of the functional layer on the surface and inside of the laser additive functional layer, which meets the technical requirements.
[0048] The spinning mold that passed the above inspection was put on the machine for testing. The spinning force was 50 tons, and the wall thickness reduction of each spinning pass was not less than 1.5mm. The results are shown in Table 2.
[0049] Table 2 Usage test results serial number Laser additive manufacturing spinning produces 300 parts Cold working die steel spinning production 300 pieces M403 type example 1 No surface defects No surface defects M632 Model 1 No surface defects No surface defects M403 type example 2 No surface defects No surface defects M632 Model 2 No surface defects No surface defects From the results in Table 2, it can be seen that the use of the M403 and M632 spinning dies made in the embodiment of the present invention is equivalent to the use of the spinning dies made of cold working die steel, and both can meet the requirements of spinning operations. Since the raw materials of cold working die steel are Cr12MoV or 70Cr3NiMo, the raw material cost is high and the overall processing technology is complicated. In comparison, the comprehensive cost of laser additive manufacturing is reduced by about 20% compared with the comprehensive manufacturing cost of cold working die steel, and the manufacturing cycle is reduced by 30%.
[0050] It should be noted that in actual use tests, 300 workpieces were spun without defects using the M403 and M632 spinning dies made in the embodiments of the present invention. Combined with the data analysis of the surface hardness and the depth of the overall hardened layer in Table 1, the overall service life of the spinning die made by the method of Example 2 will be greater than that of Example 1, which is equivalent to the performance of cold working die steel.
[0051] The present invention adopts the laser additive manufacturing method to manufacture the spinning mold, the process is stable and reliable, the quality is controllable, and cyclic repair can be achieved, which greatly improves the recycling of raw materials and reduces the cost of material scrapping.
[0052] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0053] The above is a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed by the present invention, and these modifications or replacements should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.
Claims
1. A method for making a spinning mold using laser additive technology, characterized in that: The following steps are involved: S1. Performing laser additive manufacturing on the surface of the forging blank to be processed to obtain a mold precursor; S2, heat treating the mold precursor to obtain a spinning mold; The laser additive process parameters in step S1 include: a linear speed of 20 to 70 mm / s; an overlap rate of 35 to 50%; and a laser power of 3000 to 6000 W.
2. The method for making a spinning mold using laser additive technology according to claim 1, characterized in that: The powder used in the laser additive manufacturing in step S1 is at least one of die steel and high-speed steel alloy.
3. The method for making a spinning mold using laser additive technology according to claim 1, characterized in that: The thickness of the laser added material in step S1 is 3 to 8 mm.
4. The method for making a spinning mold using laser additive technology according to claim 1, characterized in that: In the step S1, the thickness of a single layer of laser additive is 0.3-1.4 mm.
5. The method for making a spinning mold using laser additive technology according to claim 1, characterized in that: In step S2, the heat treatment process includes quenching and high-temperature tempering; wherein the quenching temperature is 950-1050°C, and the high-temperature tempering temperature is 510-520°C.
6. The method for making a spinning mold using laser additive technology according to claim 5, characterized in that: The heat treatment process also includes stress relief annealing, and the stress relief annealing temperature is 220-280°C.
7. The method for making a spinning mold using laser additive technology according to claim 6, characterized in that: The specific process of the heat treatment is to keep the temperature at the stress relief annealing temperature for 4 to 10 hours, then keep the temperature at the quenching temperature for 4 to 8 hours and then oil cool, and then keep the temperature at the high temperature tempering temperature for not less than 4 hours.
8. The method for manufacturing a spinning mold using laser additive technology according to any one of claims 5 to 7, characterized in that: The quenching is performed 1 to 3 times, and the high temperature tempering is performed 1 to 3 times.
9. The method for making a spinning mold using laser additive technology according to claim 1, characterized in that: The material of the forging blank is alloy structural steel.
10. A spinning die, characterized in that: The spinning die is prepared by the preparation method according to any one of claims 1 to 9, wherein the surface hardness of the spinning die is above 60HRC, and the depth of the hardened layer is 25 to 30 mm.
Citation Information
Patent Citations
High-wear-resistance die steel product for hot stamping and additive manufacturing process of high-wear-resistance die steel product
CN114427091A
Method for preparing high-ductility and high-toughness 1CrMo alloy repair layer through laser additive and post-heat treatment composite technology
CN115351292A
Machining method of spinning core mold for thin-wall cylindrical part
CN115786904A
Spinning roller surface laser reinforced processing forming method
US20180333802A1
KR20200117587A