Tungsten-tantalum-nickel-titanium-vanadium alloy and preparation method and application thereof

By adding tantalum and vanadium elements to the tungsten alloy for solid solution strengthening and fine crystal strengthening, combining nickel-titanium as the bonding phase, and using molding and vacuum sintering processes, the performance reduction caused by intermetallic compounds in existing tungsten alloys is solved. , achieves high strength and high toughness, is suitable for industrial production, and broadens the scope of application.

CN119035530AActive Publication Date: 2024-11-29CENT SOUTH UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411146807.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

After the existing tungsten alloy system adds solid solution elements, the matrix phase and solid solution elements form a large number of intermetallic compounds, consume solid solution elements, and reduce solid solubility. The intermetallic compounds are hard and brittle phases, which greatly reduces the alloy properties.

Method used

Solid solution strengthening and fine crystal strengthening are used to adopt tantalum and orderly phases to increase the strength of tungsten particles, and reduce the elastic modulus through vanadium and improve ductility. Nickel-titanium is used as the bonding phase to ensure solid solution elements The effective solid solution is combined with molding and vacuum sintering processes to achieve the densification of the alloy.

Benefits of technology

The densification of alloys is achieved at lower temperatures, improving the strength and toughness of the alloy, extending service life, and broadening the application range of tantalum alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035530A_ABST
    Figure CN119035530A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of tungsten alloy preparation, and particularly relates to a tungsten-tantalum-nickel-titanium-vanadium alloy and a preparation method and application thereof. The alloy comprises tungsten, tantalum, nickel, titanium and vanadium according to the mass ratio of (120-200): (10-40): (10-40): (2-18). The preparation method comprises the steps that tungsten powder, tantalum powder, nickel-titanium alloy powder and vanadium powder are mixed to obtain mixed powder, and the mixed powder is subjected to compression molding and vacuum sintering densification. The nickel-titanium alloy powder is used as a binding phase, so that strengthening and toughening of tungsten particles by the tantalum element and the vanadium element are realized, and the mechanical property of the tungsten alloy is improved. The developed and prepared tungsten-tantalum-nickel-titanium-vanadium alloy can be used as a radiation shielding device, a bullet core of an armor-piercing bullet, a bullet shell of an energy-gathered bullet, a rotor body on the outer edge of a gyroscope and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of tungsten alloy preparation, and specifically relates to a tungsten-tantalum-nickel-titanium-vanadium alloy and a preparation method and application thereof. Background Art

[0002] Tungsten (W) was first discovered by humans in the 18th century. As a strategic metal, W is widely used in modern industry, national defense and high-tech fields due to its high density, high strength, high hardness, excellent electrical and thermal conductivity. The development of science and technology has put forward higher requirements on the strength and toughness of tungsten.

[0003] The addition of tantalum can effectively improve the performance of tungsten alloys by solid solution strengthening. Tantalum, like tungsten, belongs to the body-centered cubic (BCC) structure and can be infinitely dissolved with tungsten. The ordered phase formed in the tungsten-tantalum solid solution can improve the change of the symmetrical nuclear structure of tungsten, increase the mobility of dislocations, and improve the performance of tungsten particles. At the same time, the addition of tantalum can reduce the solubility of tungsten in the bonding phase, playing a role in fine grain strengthening. The addition of vanadium can effectively reduce the elastic modulus of W and improve the ductility of the alloy.

[0004] After adding the solid solution elements to the current tungsten alloy system (W-Ni-Fe, W-Ni-Cu), the matrix phase will form a large number of intermetallic compounds with the solid solution elements. These intermetallic compounds not only consume the solid solution elements and reduce the solubility of the solid solution elements in the tungsten particles, but most of the intermetallic compounds are hard and brittle phases, which greatly reduces the performance of the alloy. Using nickel and titanium as the bonding phase of the alloy can effectively strengthen the tungsten particles by solid solution elements. Summary of the invention

[0005] Aiming at the deficiencies in the prior art. The first object of the present invention is to provide a solid solution strengthened tungsten-tantalum-nickel-titanium-vanadium alloy. The addition of tantalum can introduce an ordered phase into the tungsten crystal to produce solid solution strengthening, while reducing the dissolution and precipitation of tungsten in the binder phase to produce fine grain strengthening and improve the strength of the alloy; by adding vanadium, the elastic modulus of W is reduced and the ductility is improved. The use of nickel titanium as the binder phase ensures that tantalum and vanadium are solid-dissolved into the tungsten particles to produce a synergistic strengthening effect.

[0006] The second object of the present invention is to provide a method for preparing a tungsten-tantalum-nickel-titanium-vanadium alloy, which can achieve densification of the alloy at a relatively low temperature, has the advantages of a simple process flow and a short production cycle, and is suitable for industrial production.

[0007] The third object of the present invention is to provide an application of tungsten-tantalum-nickel-titanium-vanadium alloy, which can be used as a raw material in radiation shielding, counterweights and the outer edge rotor body of a gyroscope of a large-caliber kinetic penetrator, thereby greatly extending its service life.

[0008] The present invention discloses a tungsten-tantalum-nickel-titanium-vanadium alloy. In the alloy, the mass ratio of tungsten, tantalum, nickel titanium and vanadium is 120-200:10-40:10-40:2-18.

[0009] The invention discloses a method for preparing a tungsten-tantalum-nickel-titanium-vanadium alloy. The alloy is prepared by mixing tungsten powder, tantalum powder, vanadium powder and nickel-titanium alloy powder to obtain a mixed powder, pressing the mixed powder to obtain a compact, and sintering the compact in a vacuum environment.

[0010] As a preferred solution, the mass ratio of the tungsten powder, tantalum powder, nickel-titanium alloy powder and vanadium powder is 120-200:10-40:10-40:2-18, preferably 140-175:12-30:20-30:3-12, and further preferably: 145-170:15-30:22-28:4-11.

[0011] When used in industry, the mass ratio of the tungsten powder, tantalum powder, nickel-titanium alloy powder and vanadium powder is further preferably 150-165:16-28.5:24-26:4.5-10.5, including the scheme that the mass ratio of tungsten powder, tantalum powder, nickel-titanium alloy powder and vanadium powder is 160-164:16-20:18-22:8-12, and also including the scheme that the mass ratio of tungsten powder, tantalum powder, nickel-titanium alloy powder and vanadium powder is 150-154:27-28.5:24-26:4.5-5.5.

[0012] As one of the best limited solutions, the mass ratio of tungsten powder, tantalum powder, nickel-titanium alloy powder and vanadium powder is 160-164:16-20:18-22:8-12, including the mass ratio of tungsten powder, tantalum powder, nickel-titanium alloy powder and vanadium powder is 162:18:20:10.

[0013] As one of the best limited solutions, the mass ratio of tungsten powder, tantalum powder, nickel-titanium alloy powder and vanadium powder is 150-154:27-28.5:24-26:4.5-5.5, including the mass ratio of tungsten powder, tantalum powder, nickel-titanium alloy powder and vanadium powder is 152:28:25:5.

[0014] In the nickel-titanium alloy powder, the mass ratio of nickel to titanium is (45-55):(45-55).

[0015] The invention discloses a method for preparing a tungsten-tantalum-nickel-titanium-vanadium alloy. The method comprises the following steps: uniformly mixing tungsten powder, tantalum powder, vanadium powder and nickel-titanium alloy powder taken according to a set composition to obtain a mixed powder, and then subjecting the mixed powder to molding to obtain a pressed green sheet and vacuum sintering to obtain the mixed powder.

[0016] The key to the preparation method of the present invention is to add an appropriate amount of tantalum that can achieve infinite solid solution with tungsten. The ordered phase formed in the tungsten-tantalum solid solution can improve the change of the symmetrical nuclear structure of tungsten, improve the strength of tungsten particles, and reduce the solubility of tungsten in the matrix phase, hinder the dissolution and precipitation process of tungsten particles, refine the tungsten particles, and play a role in fine grain strengthening. Adding too much tantalum powder has no positive effect on the overall strength. During the sintering process, the oxygen in the tantalum powder will be adsorbed by titanium to generate titanium oxide particles, destroying the bonding phase structure and reducing the mechanical properties of the alloy.

[0017] At the same time, vanadium is added to improve the ductility of the alloy, further improving the machinability of the alloy. The addition of trace vanadium does not affect the microstructure and organizational homogeneity of the alloy.

[0018] It was discovered that carrying out preliminary weighing work in a vacuum glove box can effectively reduce the oxidation of tungsten and tantalum during the mixing process, reduce the loss of titanium during sintering, and reduce the formation of metal compound.

[0019] As a preferred solution, the tungsten powder is a spherical powder with an average particle size of 3 to 5 μm and a purity of 99.8% or more; the tantalum powder is a spherical powder with an average particle size of 3 to 10 μm and a purity of 99.9% or more; the rhenium powder is a spherical powder with an average particle size of 3 to 10 μm and a purity of 99.9% or more. The raw materials used in the present invention are all spherical powders, because spherical powders have the highest specific surface area under the same mass, can provide the highest sintering activity, and improve the diffusion capacity between elements.

[0020] As a preferred solution, the mixing is carried out in a three-dimensional mixer for 12 to 14 hours. A uniformly mixed tungsten, tantalum, nickel, titanium and vanadium powder can be obtained by mixing in a three-dimensional mixer.

[0021] After mixing, the mass percentage of oxygen in the uniformly mixed tungsten, tantalum, nickel, titanium and vanadium powders is less than or equal to 600 ppm.

[0022] As a preferred solution, the compression molding method is die compression molding. The present invention obtains reliable dense green compacts by die compression molding.

[0023] As a preferred solution, the compression molding method is die compression molding, the molding pressure is 450MPa-650MPa, preferably 480-520MPa, and the holding time is 5-10s. In the technical solution of the present invention, if the molding pressure value is too low, the edge of the powder compact cannot be formed, and if the pressure value is too high, the compact will be delaminated, so the maximum pressure should not exceed 650MPa.

[0024] As a preferred solution, the vacuum degree during sintering is ≤10 -3Pa; Since titanium easily absorbs oxygen, the vacuum degree needs to be strictly controlled during the sintering process of tungsten-tantalum-nickel-titanium-vanadium alloy to avoid oxidation during the sintering process.

[0025] As a preferred solution, the sintering process is: heating to 800-1000°C, preferably 850-900°C, at a heating rate of 5-20°C / min, and keeping warm for 10-40min; then heating to 1100-1200°C, preferably 1100-1150°C, at a cooling rate of 2-10°C / min, and keeping warm for 60-300min; then heating to 1300-1400°C, preferably 1300-1350°C, at a heating rate of 2-10°C / min, and keeping warm for 30-90min; finally cooling to room temperature at a cooling rate of 5-35°C / min. The technical solution of the present invention first heats the alloy powder to 800-1000°C, so that a preliminary sintering neck is formed between the powders, and on the other hand, the temperature in the furnace can be stabilized. Further increasing the sintering temperature to 1300-1400°C can quickly achieve densification of the embryo. At the same time, keeping the temperature between 1100 and 1200°C can further improve the uniformity of the alloy structure and the mechanical properties of the alloy.

[0026] The present invention also provides a tungsten-tantalum-nickel-titanium-vanadium alloy obtained by the above preparation method. The tungsten-tantalum-nickel-titanium-vanadium alloy is solid-solution strengthened by tantalum and vanadium elements, has no intermetallic compound, and the particle size of the alloy matrix is ​​≤20 μm.

[0027] In a preferred solution, the tensile strength of the tungsten-tantalum-nickel-titanium-vanadium alloy is greater than or equal to 800 MPa (can be greater than or equal to 970 MPa after optimization), and the tensile strain is greater than 15%.

[0028] The present invention also provides an application of a tungsten-tantalum-nickel-titanium-vanadium alloy, which is used as a raw material for radiation shielding, counterweights, and the outer edge rotor body of a gyroscope of a large-caliber kinetic penetrator, which can not only greatly improve its service life, but also greatly broaden the application scope of the tantalum alloy.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] 1) The alloy system of the present invention uses tantalum to strengthen tungsten particles, supplemented by an appropriate amount of vanadium to improve the toughness of the alloy. After the two solid solution elements are added in combination, the strength and toughness of the alloy are improved. The strength of the alloy increases with the increase of the tantalum content, but with the further increase of the vanadium content, the change in toughness is not obvious. Under the synergistic effect of the two elements, the sintered body shows good strength and toughness. The alloy designed by the present invention can prepare a tungsten-tantalum-rhenium alloy with a strength of more than 970MPa.

[0031] 2) The present invention uses a three-dimensional mixer to add the solid solution element tantalum and performs compression molding; the designed alloy system successfully achieves solid solution strengthening of tungsten under the traditional sintering mode.

[0032] 3) The tungsten-tantalum-nickel-titanium-vanadium alloy provided by the present invention can be used for radiation shielding, counterweights, large-caliber kinetic penetrators, gyroscope outer rotor bodies, etc., which greatly broadens the application of tantalum alloys. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is the original morphology of the tungsten element powder, tantalum element powder, vanadium element powder and nickel-titanium alloy powder used in Example 1.

[0034] Figure 2 This is a morphology diagram of the tungsten-tantalum-nickel-titanium-vanadium alloy obtained in Example 1;

[0035] Figure 3 This is a morphology image of the tungsten-tantalum-nickel-titanium-vanadium alloy obtained in Example 2;

[0036] Figure 4 This is a morphology image of the tungsten-tantalum-nickel-titanium-vanadium alloy obtained in Example 3;

[0037] Figure 5 This is a morphology image of the tungsten-tantalum-nickel-titanium-vanadium alloy obtained in Example 4;

[0038] Figure 6 This is a morphology image of the tungsten-tantalum-nickel-titanium-vanadium alloy obtained in Example 5;

[0039] Figure 7 The macroscopic morphologies of Comparative Examples 2 and 3 after compression molding, wherein (a) is the macroscopic morphology of Comparative Example 2 after compression molding, and (b) is the macroscopic morphology of Comparative Example 3 after compression molding.

[0040] Figure 8 Statistical graphs of the tensile strength and average relative density of the tungsten-tantalum-nickel-titanium-vanadium alloys obtained in Example 1, Example 2, Example 3, Example 4, Example 5, Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4.

[0041] Figure 1 Depend on Figure 1 (a) Figure 1 (b) Figure 1 (c) Figure 1 (d) Composition. Figure 1 (a) is the morphology of tungsten powder. Figure 1 (b) is the morphology of tantalum powder. Figure 1 (c) is the morphology of vanadium powder. Figure 1 (d) is the morphology of the mixed powder. Figure 1It can be seen that the W powder is in the shape of an equiaxed polyhedron, the Ta powder and the V powder are mostly in the shape of irregular polygons, and the NiTi alloy powder is in the shape of a regular sphere.

[0042] Figure 2 The morphology of the tungsten-tantalum-nickel-titanium-vanadium alloy prepared in Example 1 is compared with Figure 3 It can be seen that the reduction of sintering time and sintering temperature makes the distribution of the binder phase uneven, a large molten pool appears, and the uniformity of the material is reduced, resulting in the reduction of alloy performance.

[0043] from Figure 2 , Figure 3 , Figure 4 , Figure 5 Obvious liquid phase sintering characteristics can be observed.

[0044] from Figure 6 It can be seen that in Example 6, since the sintering temperature is too low, the dissolution and precipitation of tungsten particles is not sufficient.

[0045] Figure 7 (a) shows the forming condition of the embryo when the pressure is too low during the powder forming process. It can be observed that the edge of the embryo is irregular, a large amount of powder is separated from the embryo, and the overall density is low after sintering. Figure 7 (b) shows the forming condition of the embryo when the pressure is too high during the powder forming process, and the embryo is stratified as a whole.

[0046] Figure 8 It can be found that the performance of the alloy has been significantly improved due to the addition of vanadium. However, the excessive addition of V element makes the proportion of NiTi as a liquid phase component insufficient, the ability to dissolve W particles becomes poor, and the lack of bonding phase leads to excessive tungsten-tungsten connection, which greatly reduces the mechanical properties of the alloy. DETAILED DESCRIPTION

[0047] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.

[0048] Example 1

[0049] A method for preparing a tungsten-tantalum-nickel-titanium-vanadium alloy comprises the following steps:

[0050] Step 1: Use a three-dimensional mixer to obtain mixed powder

[0051] In a vacuum glove box, take 162g of tungsten powder, with an average particle size of 3 to 5 microns and a purity greater than 99.8%; 18g of tantalum powder, with an average particle size of 3 to 10 microns and a purity greater than 99.9%; take 5g of vanadium powder, with an average particle size of 3 to 10 microns and a purity greater than 99.9%; take 25g of nickel-titanium alloy powder (in the nickel-titanium alloy powder, the mass ratio of nickel to titanium is 55:45), with an average particle size of 5 to 23 microns and a purity greater than 99.9%, and put the above powders together into a tungsten carbide mixing tank. Take the mixing tank out of the vacuum glove box and put it into a three-dimensional mixer for 12 hours of mixing (after mixing, the mass percentage of oxygen is less than or equal to 500ppm).

[0052] Step 2: Use compression molding to obtain the green body

[0053] 180 g of the mixed powder was placed in a mold and pressed at a pressure of 500 MPa for 5 s.

[0054] Step 3: Sintering of Tungsten-Tantalum-Nickel-Titanium-Vanadium Alloy

[0055] The sintering process uses the AL-2000-MG high vacuum heat treatment furnace of Sichuan Liye Technology Co., Ltd. During the sintering process, the vacuum degree in the furnace is maintained at 10 -3 The temperature was raised to 900°C at a heating rate of 10°C / min, kept warm for 30 min, then raised to 1200°C at a heating rate of 5°C / min, kept warm for 180 min, then raised to 1320°C at a heating rate of 5°C / min, kept warm for 120 min, and then cooled to room temperature at 20°C / min to obtain a tungsten-tantalum-nickel-titanium-vanadium alloy.

[0056] The tungsten-tantalum-nickel-titanium-vanadium alloy prepared in this embodiment has an average relative density of 98.0%, a tensile strength of 924 MPa, and a total elongation of 9.5%.

[0057] Example 2

[0058] Step 1: Use a three-dimensional mixer to obtain mixed powder

[0059] In a vacuum glove box, take 162g of tungsten powder, with an average particle size of 3 to 5 microns and a purity greater than 99.8%; 18g of tantalum powder, with an average particle size of 3 to 10 microns and a purity greater than 99.9%; take 5g of vanadium powder, with an average particle size of 3 to 10 microns and a purity greater than 99.9%; take 25g of nickel-titanium alloy powder (in the nickel-titanium alloy powder, the mass ratio of nickel to titanium is 55:45), with an average particle size of 5 to 23 microns and a purity greater than 99.9%, and put the above powders together into a tungsten carbide mixing tank. Take the mixing tank out of the vacuum glove box and put it into a three-dimensional mixer for 12 hours of mixing (after mixing, the mass percentage of oxygen is less than or equal to 500ppm).

[0060] Step 2: Use compression molding to obtain the green body

[0061] 180 g of the mixed powder was placed in a mold and pressed at a pressure of 500 MPa for 5 s.

[0062] Step 3: Sintering of Tungsten-Tantalum-Nickel-Titanium-Vanadium Alloy

[0063] The sintering process uses the AL-2000-MG high vacuum heat treatment furnace of Sichuan Liye Technology Co., Ltd. During the sintering process, the vacuum degree in the furnace is maintained at 10 -3 The temperature was raised to 800°C at a heating rate of 10°C / min, and kept warm for 30 min. The temperature was then raised to 1200°C at a heating rate of 5°C / min, and kept warm for 60 min. The temperature was then raised to 1300°C at a heating rate of 5°C / min, and kept warm for 120 min. The furnace was then cooled to room temperature to obtain a tungsten-tantalum-nickel-titanium-vanadium alloy.

[0064] The tungsten-tantalum-nickel-titanium-vanadium alloy prepared in this embodiment has an average relative density of 93.2%, a tensile strength of 902 MPa, and a total elongation of 9.0%.

[0065] Example 3

[0066] Step 1: Use a three-dimensional mixer to obtain mixed powder

[0067] In a vacuum glove box, take 162g of tungsten powder, with an average particle size of 3 to 5 microns and a purity greater than 99.8%; 18g of tantalum powder, with an average particle size of 3 to 10 microns and a purity greater than 99.9%; take 10g of vanadium powder, with an average particle size of 3 to 10 microns and a purity greater than 99.9%; take 20g of nickel-titanium alloy powder (in the nickel-titanium alloy powder, the mass ratio of nickel to titanium is 55:45), with an average particle size of 5 to 23 microns and a purity greater than 99.9%, and put the above powders together into a tungsten carbide mixing tank. Take the mixing tank out of the vacuum glove box and put it into a three-dimensional mixer for 12 hours of mixing (after mixing, the mass percentage of oxygen is less than or equal to 500ppm).

[0068] Step 2: Use compression molding to obtain the green body

[0069] 180 g of the mixed powder was placed in a mold and pressed at a pressure of 500 MPa for 5 s.

[0070] Step 3: Sintering of Tungsten-Tantalum-Nickel-Titanium-Vanadium Alloy

[0071] The sintering process uses the AL-2000-MG high vacuum heat treatment furnace of Sichuan Liye Technology Co., Ltd. During the sintering process, the vacuum degree in the furnace is maintained at 10 -3The temperature was raised to 900°C at a heating rate of 10°C / min, kept warm for 30 min, then raised to 1200°C at a heating rate of 5°C / min, kept warm for 180 min, then raised to 1320°C at a heating rate of 5°C / min, kept warm for 120 min, and then cooled to room temperature at 20°C / min to obtain a tungsten-tantalum-nickel-titanium-vanadium alloy.

[0072] The tungsten-tantalum-nickel-titanium-vanadium alloy prepared in this embodiment has an average relative density of 98.6%, a tensile strength of 966 MPa, and a total elongation of 10.1%.

[0073] Example 4

[0074] A method for preparing a tungsten-tantalum-nickel-titanium-vanadium alloy comprises the following steps:

[0075] Step 1: Use a three-dimensional mixer to obtain mixed powder

[0076] In a vacuum glove box, take 152g of tungsten powder, with an average particle size of 3 to 5 microns and a purity greater than 99.8%; 28g of tantalum powder, with an average particle size of 3 to 10 microns and a purity greater than 99.9%; 5g of vanadium powder, with an average particle size of 3 to 10 microns and a purity greater than 99.9%; and 25g of nickel-titanium alloy powder, with an average particle size of 5 to 23 microns and a purity greater than 99.9%, and put the above powders together into a tungsten carbide mixing tank. Take the mixing tank out of the vacuum glove box and put it into a three-dimensional mixer for 12 hours of mixing (after mixing, the mass percentage of oxygen is less than or equal to 500ppm).

[0077] Step 2: Use compression molding to obtain the green body

[0078] 180 g of the mixed powder was placed in a mold and pressed at a pressure of 500 MPa for 5 s.

[0079] Step 3: Sintering of Tungsten-Tantalum-Nickel-Titanium-Vanadium Alloy

[0080] The sintering process uses the AL-2000-MG high vacuum heat treatment furnace of Sichuan Liye Technology Co., Ltd. During the sintering process, the vacuum degree in the furnace is maintained at 10 -3 The temperature was raised to 900°C at a heating rate of 10°C / min, and kept warm for 30 min. The temperature was then raised to 1200°C at a heating rate of 5°C / min, and kept warm for 180 min. The temperature was then lowered to 1320°C at a cooling rate of 5°C / min, and kept warm for 120 min. The alloy was then cooled to room temperature to obtain a tungsten-tantalum-nickel-titanium-vanadium alloy.

[0081] The tungsten-tantalum-nickel-titanium-vanadium alloy prepared in this embodiment has an average relative density of 98.1%, a tensile strength of 982 MPa, and a total elongation of 10.9%.

[0082] Example 5

[0083] A method for preparing a tungsten-tantalum-nickel-titanium-vanadium alloy comprises the following steps:

[0084] Step 1: Use a three-dimensional mixer to obtain mixed powder

[0085] In a vacuum glove box, take 162g of tungsten powder, with an average particle size of 3 to 5 microns and a purity greater than 99.8%; 18g of tantalum powder, with an average particle size of 3 to 10 microns and a purity greater than 99.9%; take 5g of vanadium powder, with an average particle size of 3 to 10 microns and a purity greater than 99.9%; take 25g of nickel-titanium alloy powder (in the nickel-titanium alloy powder, the mass ratio of nickel to titanium is 55:45), with an average particle size of 5 to 23 microns and a purity greater than 99.9%, and put the above powders together into a tungsten carbide mixing tank. Take the mixing tank out of the vacuum glove box and put it into a three-dimensional mixer for 12 hours of mixing (after mixing, the mass percentage of oxygen is less than or equal to 500ppm).

[0086] Step 2: Use compression molding to obtain the green body

[0087] 180 g of the mixed powder was placed in a mold and pressed at a pressure of 500 MPa for 5 s.

[0088] Step 3: Sintering of Tungsten-Tantalum-Nickel-Titanium-Vanadium Alloy

[0089] The sintering process uses the AL-2000-MG high vacuum heat treatment furnace of Sichuan Liye Technology Co., Ltd. During the sintering process, the vacuum degree in the furnace is maintained at 10 -3 The temperature was raised to 900°C at a heating rate of 10°C / min, and kept warm for 30 min. The temperature was then raised to 1000°C at a heating rate of 5°C / min, and kept warm for 180 min. The temperature was then raised to 1200°C at a heating rate of 5°C / min, and kept warm for 120 min. The temperature was then cooled to room temperature at a heating rate of 20°C / min to obtain a tungsten-tantalum-nickel-titanium-vanadium alloy.

[0090] The tungsten-tantalum-nickel-titanium-vanadium alloy prepared in this embodiment has an average relative density of 98.0%, a tensile strength of 346 MPa, and a total elongation of 2.5%.

[0091] Comparative Example 1

[0092] The other conditions of this comparative example are the same as those of Example 1, except for step 1: in a vacuum glove box, take 162g of tungsten powder, with an average particle size of 3 to 5 microns and a purity greater than 99.8%; 18g of tantalum powder, with an average particle size of 3 to 10 microns and a purity greater than 99.9%; take 30g of nickel-titanium alloy powder, with an average particle size of 5 to 23 microns and a purity greater than 99.9%, and put the above powders together into a tungsten carbide mixing tank. Take the mixing tank out of the vacuum glove box and put it into a three-dimensional mixer for 12 hours of mixing (after mixing, the mass percentage of oxygen is less than or equal to 500ppm).

[0093] The material prepared in this comparative example has an average relative density of 97.6%, a tensile strength of 810 MPa, and a total elongation of 9.2%.

[0094] Comparative Example 2

[0095] The other conditions of this comparative example are the same as those of Example 1, except for step 2: 180 g of the mixed powder is placed in a mold and pressed at a pressure of 300 MPa for 5 seconds.

[0096] The material prepared in this comparative example has an average relative density of 88.6%, a tensile strength of 870 MPa, and a total elongation of 9.5%.

[0097] Comparative Example 3

[0098] The other conditions of this comparative example are the same as those of Example 1, except for step 2: 180 g of the mixed powder is placed in a mold and pressed at a pressure of 600 MPa for 5 seconds.

[0099] The material prepared in this comparative example has an average relative density of 98%, a tensile strength of 912 MPa, and a total elongation of 10.1%.

[0100] Comparative Example 4

[0101] The other conditions of this comparative example are the same as those of Example 1, except for step 1: in a vacuum glove box, take 162g of tungsten powder, with an average particle size of 3 to 5 microns and a purity greater than 99.8%; 18g of tantalum powder, with an average particle size of 3 to 10 microns and a purity greater than 99.9%; take 20g of vanadium powder, with an average particle size of 3 to 10 microns and a purity greater than 99.9%; take 10g of nickel-titanium alloy powder (in the nickel-titanium alloy powder, the mass ratio of nickel to titanium is 55:45), with an average particle size of 5 to 23 microns and a purity greater than 99.9%, and put the above powders together into a tungsten carbide mixing tank. Take the mixing tank out of the vacuum glove box and put it into a three-dimensional mixer for 12 hours of mixing (after mixing, the mass percentage of oxygen is less than or equal to 500ppm).

[0102] The material prepared in this comparative example has an average relative density of 97.6%, a tensile strength of 410 MPa, and a total elongation of 2.2%.

Claims

1. A tungsten-tantalum-nickel-titanium-vanadium alloy, characterized in that: In the alloy, the mass ratio of tungsten, tantalum, nickel-titanium and vanadium is 120-200:10-40:10-40:2-18; the mass ratio of nickel to titanium is (45-55):(45-55).

2. A method for preparing a tungsten-tantalum-nickel-titanium-vanadium alloy, characterized in that: Tungsten powder, tantalum powder, vanadium powder and nickel-titanium alloy powder are mixed to obtain mixed powder, the mixed powder is pressed into a green compact, and the green compact is sintered under a vacuum environment; the mass ratio of the tungsten powder, tantalum powder, nickel-titanium alloy powder and vanadium powder is 120-200:10-40:10-40:2-18; in the nickel-titanium alloy powder, the mass ratio of nickel to titanium is (45-55):(45-55).

3. The method for preparing the tungsten-tantalum-nickel-titanium-vanadium alloy according to claim 1, characterized in that: The mass ratio of the tungsten powder, tantalum powder, nickel-titanium alloy powder and vanadium powder is 140-175:12-30:20-30:3-12.

4. The method for preparing the tungsten-tantalum-nickel-titanium-vanadium alloy according to claim 3, characterized in that: The mass ratio of the tungsten powder, tantalum powder, nickel-titanium alloy powder and vanadium powder is 145-170:15-30:22-28:4-11.

5. The method for preparing the tungsten-tantalum-nickel-titanium-vanadium alloy according to claim 4, characterized in that: The mass ratio of the tungsten powder, tantalum powder, nickel-titanium alloy powder and vanadium powder is 160-164:16-20:18-22:8-12; or the mass ratio of the tungsten powder, tantalum powder, nickel-titanium alloy powder and vanadium powder is 150-154:27-28.5:24-26:4.5-5.

5.

6. The method for preparing a tungsten-tantalum-nickel-titanium-vanadium alloy according to claim 2, characterized in that: The tungsten powder has an average particle size of 3 to 5 μm and a purity of ≧99.8%; The average particle size of the tantalum powder is 3 to 10 μm, and the purity is ≧99.9%; The nickel-titanium alloy powder has an average particle size of 5 to 20 μm and a purity of ≧99.9%; The average particle size of the vanadium powder is 3-5 μm, and the purity is ≧99.9%.

7. The method for preparing a tungsten-tantalum-nickel-titanium-vanadium alloy according to claim 2, characterized in that: The raw materials are mixed in a vacuum atmosphere or a protective atmosphere, and the mixed raw materials are mixed in a three-dimensional mixer for 10 to 16 hours to obtain a uniformly mixed powder.

8. The method for preparing a tungsten-tantalum-nickel-titanium-vanadium alloy according to claim 2, characterized in that: The compression molding method is die compression molding, the molding pressure is 450MPa-650MPa, and the holding time is 5-10s.

9. The method for preparing a tungsten-tantalum-nickel-titanium-vanadium alloy according to claim 2, characterized in that: The vacuum degree during sintering is ≤10 -3 Pa; the sintering process is: heating to 800-1000°C at a heating rate of 5-20°C / min, and keeping warm for 10-40min; then heating to 1100-1200°C at a cooling rate of 2-10°C / min, and keeping warm for 60-300min; then heating to 1300-1400°C at a heating rate of 2-10°C / min, and keeping warm for 30-90min; finally cooling to room temperature at a cooling rate of 5-35°C / min.

10. An application of the tungsten-tantalum-nickel-titanium-vanadium alloy as claimed in claim 1, characterized in that: The applications include at least one of being used as a radiation shield, an armor-piercing projectile core, a shaped-charge projectile shell, and a gyroscope outer rotor body.

Citation Information

Patent Citations

  • Method for preparing tungsten-based alloy

    CN101967577A

  • Five tungsten-based high-entropy alloys and preparation method thereof

    CN111254339A

  • Precipitation strengthening high-entropy alloy component design and preparation method based on diffusion multi-section technology

    CN114438391A

  • High-density tungsten alloy with high adiabatic shear sensitivity and high plasticity and preparation method of high-density tungsten alloy

    CN116240437A

  • High-density tungsten-titanium nickel alloy and preparation method thereof

    CN117187654A