Method for preparing nano nickel powder by adding reducing agent in controlled manner

By controlling the addition of reducing agent, the reducing agent was added in three times and compounds such as ethylene glycol and sodium hydroxide were used to solve the problem of uneven particle size distribution and agglomeration of nano nickel powder, and the dispersion and production efficiency of nano nickel powder were improved. , suitable for industrial production.

CN119035532AInactive Publication Date: 2024-11-29JIYUAN XINGHAN NEW MATERIAL TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411248731.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art, the particle size distribution of nano nickel powders is uneven and prone to agglomeration, resulting in poor dispersion and effective surface area, which affects material performance.

Method used

Using the method of controlling the addition of reducing agents, gradually add the reducing agent in three times to manage the particle size distribution, use compounds such as glycol and sodium hydroxide, combined with polyvinylpyrrolelenone dispersant, control the pH and temperature of the reaction solution to avoid the secondary Reaction, add reducing agents in pouring to reduce agglomeration.

Benefits of technology

It significantly improves the particle size uniformity and dispersion of nano nickel powder, improves production efficiency and product quality, reduces production costs, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035532A_ABST
    Figure CN119035532A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of battery slurry fineness detection methods, in particular to a method for preparing nano nickel powder by adding a reducing agent in a controlled mode, and the method comprises the following steps that nickel salt, ethylene glycol and a dispersing agent are mixed and stirred to prepare a nickel salt solution; mixing sodium hydroxide, ethylene glycol and a reducing agent to prepare a reducing agent solution; adding 1 / 3 of the reducing agent solution into the nickel salt solution, stirring and heating to prepare a solution A; adding 1 / 3 of the reducing agent solution into the solution A, stirring and heating to prepare a solution B; adding 1 / 3 of the reducing agent solution into the solution B, stirring and heating to prepare a solution C; separating the generated nano nickel powder from the solution C by using vacuum filtering equipment; and washing the separated nano nickel powder, and drying the nano nickel powder to obtain a nano nickel powder product. The nanometer nickel powder prepared through the preparation method is controllable in particle size and excellent in dispersity and stability, and the technical problems that nickel powder prepared through an existing method is uneven in particle size distribution, prone to agglomeration and poor in dispersity can be effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal nanoparticles, and in particular to a method for preparing nano nickel powder by controlled addition of a reducing agent. Background Art

[0002] As a nano-metal material, nano-nickel powder is widely used in many fields because of its unique physical and chemical properties. In the electronics industry, nano-nickel powder can be used to make conductive materials, such as conductive inks and coatings, as well as packaging materials for electronic components, which can improve product performance and reliability. In the battery industry, nano-nickel powder is used as an electrode material in lithium-ion batteries and nickel-hydrogen batteries, which can significantly improve battery capacity and cycle life. In addition, nano-nickel powder also exhibits excellent capacitance performance in supercapacitors. In the field of catalysis, nano-nickel powder is widely used as a catalyst carrier because of its high specific surface area and excellent chemical stability, especially in hydrogenation reactions in petrochemicals and organic synthesis, showing efficient catalytic activity. The magnetic properties of nano-nickel powder enable it to be used in magnetic storage devices and magnetic fluids, improving storage density and equipment performance. Nano-nickel powder also has important applications in the fields of medicine and biotechnology, such as drug carriers and medical imaging contrast agents, improving drug targeting and MRI imaging effects. In materials engineering, nano-nickel powder is used as a sintering additive and a reinforcing phase of composite materials to improve the mechanical properties and wear resistance of materials. Environmental protection and energy are also important application areas for nano nickel powder, especially in wastewater treatment and new energy materials, such as fuel cells and solar cell electrode materials, which improve energy conversion efficiency and pollution control effects. With the development of nanotechnology, the application prospects of nano nickel powder will be broader.

[0003] At present, common methods for preparing nano nickel powder include vapor deposition, liquid phase chemical reduction and electrochemical methods, etc. However, the nano nickel powder prepared in the prior art has some deficiencies in terms of uniformity of particle size, dispersibility and industrial production, etc. For example, the nano nickel powder prepared in the invention patent with patent announcement number CN 115087506 A has an uneven particle size distribution, and the particle size of the nano nickel powder is difficult to be uniformly controlled, resulting in unstable performance in practical applications; the nano nickel powder prepared in the invention patent with patent announcement number CN107552808 A has poor sphericity, and the nano particles are prone to agglomeration, which affects its dispersibility and effective surface area, thereby reducing the application performance of the material. Summary of the invention

[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing nano nickel powder by controlled addition of a reducing agent, wherein the reaction process is more controllable by gradually adding the reducing agent in three times, the particle size distribution can be better managed, the dispersibility and stability of the nano nickel powder can be improved, the agglomeration of the nano nickel powder can be reduced, the preparation efficiency can be improved and the production cost can be reduced, and the technical problems of uneven particle size distribution, easy agglomeration, poor dispersibility and effective surface area of ​​the nickel powder prepared by the existing preparation method can be effectively solved.

[0005] In order to achieve the above technical objectives, the present invention adopts the following technical solutions: The present invention provides a method for preparing nano nickel powder by controlled addition of a reducing agent, comprising the following steps: (1) Preparation of nickel salt solution: Mixing and stirring nickel salt, ethylene glycol and dispersant until they are completely dissolved to prepare a nickel salt solution; (2) Preparation of reducing agent solution: Weigh sodium hydroxide and ethylene glycol, add a reducing agent, mix well to prepare a reducing agent solution, and divide it into three equal parts by weight; (3) First addition of reducing agent: Add a portion of the reducing agent solution prepared in step (2) to the nickel salt solution prepared in step (1), keep stirring and continue heating to prepare solution A; (4) Second addition of reducing agent: Add a portion of the reducing agent solution prepared in step (2) to solution A in step (3), keep stirring and continue heating to prepare solution B; (5) The third addition of reducing agent: Add a portion of the reducing agent solution prepared in step (2) to solution B in step (4), keep stirring and continue heating to prepare solution C; (6) Separation of nano nickel powder: Using a vacuum filtration device to separate the nano nickel powder generated by the reaction from the solution C in step (4); (7) Washing and drying: The separated nano nickel powder is washed and then placed in a drying device for drying to finally obtain a nano nickel powder product.

[0006] In some possible implementations, in the above step (1), the nickel salt solution is prepared by using 150-180 parts of nickel salt, 1500-2300 parts of ethylene glycol and 32-38 parts of dispersant, calculated by weight.

[0007] In some possible implementations, in the above step (1), the nickel salt is nickel chloride, and the dispersant is polyvinyl pyrrolidone.

[0008] In some possible implementations, in the above step (2), the reducing agent solution is prepared by using 60-80 parts of sodium hydroxide, 500-900 parts of ethylene glycol and 80-100 parts of reducing agent, calculated by weight.

[0009] In some possible embodiments, in the above step (2), the reducing agent is hydrazine hydrate.

[0010] In some possible implementations, in the above step (2), hydrazine hydrate with a mass content of 60% is used.

[0011] In some possible embodiments, in the above step (3), the stirring time of the solution is 0.3-0.5 h, the heating temperature is 75-85° C., and the pH value of the solution A is controlled at 11. Exemplarily, the stirring time of the solution in step (3) can be selected to be 0.3 h, 0.4 h or 0.5 h, and the heating temperature is 75° C., 80° C. or 85° C.

[0012] In some possible embodiments, in the above step (4), the stirring time is 1 to 1.5 hours, and the heating temperature is 75 to 85° C. Exemplarily, in step (4), the stirring time is 1 hour, 1.2 hours or 1.5 hours, and the heating temperature is 75° C., 80° C. or 85° C.

[0013] In some possible embodiments, in the above step (5), the stirring time is 1 to 3 hours, and the heating temperature is 75 to 85° C. Exemplarily, in step (5), the stirring time is 1 hour, 1.5 hours, 2 hours, 2.5 hours or 3 hours, and the heating temperature is 75° C., 80° C. or 85° C.

[0014] In some possible implementations, in the above steps (3) to (5), the reducing agent solution is added by pouring, and the pouring speed is 500-1500 mL / min. Exemplarily, the pouring speed of the reducing agent solution in steps (3) to (5) is 500 mL / min, 800 mL / min, 1000 mL / min, 1200 mL / min or 1500 mL / min.

[0015] In some possible implementations, in the above step (7), the separated nano-nickel powder is washed with deionized water, and the nano-nickel powder is placed in a vacuum drying oven and dried at a drying temperature of 75-85° C., preferably 80° C.

[0016] The present invention has the following beneficial effects: The present invention makes the reaction process more controllable by gradually adding a reducing agent, can better manage the particle size distribution of the nickel powder generated by the reaction, ensure the uniformity and nanometer size of the nickel powder, significantly improve the particle size uniformity and dispersibility of the nano nickel powder, and improve production efficiency and product quality. The specific process of the present invention can be divided into three times of adding a reducing agent. The first time the reducing agent is added to control nucleation to ensure that the initial particle size is small and uniform; the second and third times the reducing agent is added to control the gradual growth of the particles respectively to avoid uneven particle size caused by too fast growth. During the entire reaction process, it is ensured that the pH and temperature of the reaction solution are maintained within a suitable range to avoid the occurrence of side reactions. The reducing agent is added to the nickel salt solution in a pouring manner, and a polyvinyl pyrrolidone (PVP) dispersant is used to help reduce the agglomeration phenomenon of the nano nickel powder and improve the dispersibility and stability of the nano nickel powder. The preparation method of the nano nickel powder provided by the present invention is simple and convenient to operate, has high preparation efficiency, and low production cost, and provides a new technical approach for the industrial production and wide application of nano materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings: Figure 1 It is a schematic flow chart of a method for preparing nano nickel powder by controlled addition of a reducing agent according to the present invention; Figure 2 is a SEM image of the nano nickel powder prepared by adding a reducing agent three times in Example 1 of the present invention; Figure 3 is a SEM image of the nano nickel powder prepared by adding the reducing agent three times in Example 2 of the present invention; Figure 4 is a SEM image of the nano nickel powder prepared by adding a reducing agent three times in Example 3 of the present invention; Figure 5 This is a SEM image of the nano nickel powder prepared by adding a reducing agent once in Comparative Example 1 of the present invention; Figure 6 is a SEM image of the nano nickel powder prepared by adding the reducing agent twice in Comparative Example 2 of the present invention; Figure 7 This is a SEM picture of the nano nickel powder prepared by adding the reducing agent four times in Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0018] The following specific embodiments illustrate the implementation of the present invention, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Although the description of the present invention will be introduced in conjunction with the preferred embodiment, it does not mean that the features of this invention are limited to the implementation.

[0019] With the rapid development of nanotechnology, nanomaterials are more and more widely used in various fields. Among them, nano nickel powder has become an important material in the fields of electronics, batteries, catalysts and composite materials due to its excellent electromagnetic properties, catalytic properties and mechanical properties. However, the preparation of nano nickel powder still has some shortcomings in terms of uniformity, dispersibility and industrial production of particle size. The common preparation method of nano nickel powder is chemical reduction method. The present invention aims to provide a kind of efficient and reliable preparation method of nano nickel powder, by adding reducing agent three times, ensuring the uniformity and nanometer size of nickel powder, significantly improving the particle size uniformity and dispersibility of nano nickel powder, and improving production efficiency and product quality.

[0020] Example: refer to Figure 1 The present invention provides a method for preparing nano nickel powder by controlled addition of a reducing agent, comprising the following steps: (1) Preparation of nickel salt solution: Weigh 150-180 parts of nickel chloride, 1500-2300 parts of ethylene glycol and 32-38 parts of PVP by mass, mix and stir until completely dissolved to prepare a nickel salt solution for later use; (2) Preparation of reducing agent solution: Weigh 60-80 parts of sodium hydroxide and 500-900 parts of ethylene glycol by mass, then add 80-100 parts of hydrazine hydrate with a mass content of 60%, mix well, and prepare a reducing agent solution for standby use; (3) First addition of reducing agent: Under stirring and heating conditions, pour 1 / 3 of the reducing agent solution into the nickel salt solution, with the stirring time being 0.3-0.5h, the heating temperature being 75-85°C, and the pH value of the solution being controlled at 11 to obtain solution A; (4) Second addition of reducing agent: Under stirring and heating conditions, pour 1 / 3 of the reducing agent solution into solution A, stir for 1-1.5 hours, and heat at 75-85°C to obtain solution B; (5) The third addition of reducing agent: Under stirring and heating conditions, pour 1 / 3 of the reducing agent solution into solution B, stir for 1-3 hours, and heat at 75-85°C to obtain solution C. (6) Separation of nano nickel powder: The nano nickel powder generated by the reaction is separated from solution C using a vacuum filtration device; (7) Washing and drying: The separated nano nickel powder is washed with deionized water, and then placed in a vacuum drying oven for drying, with the drying temperature controlled at 80° C., to finally obtain a nano nickel powder product.

[0021] In the present invention, the speeds of pouring the reducing agent solution for the first time, the second time and the third time are the same, and the pouring speed is controlled at 500-1500 mL / min.

[0022] In order to make the purpose, technical scheme and advantages of the present invention clearer, the embodiments of the present invention are described in further detail below. Unless otherwise specified in the following examples, the raw materials used are all common commercial products.

[0023] Example 1 This embodiment provides a method for preparing nano nickel powder by controlled addition of a reducing agent, comprising the following steps: (1) Preparation of nickel salt solution: Weigh 155 g of nickel chloride and 1800 g of ethylene glycol, place them in a clean beaker, stir and mix them evenly, then add 32 g of PVP to the beaker to prevent the nanoparticles from agglomerating during the reaction, stir until they are completely dissolved, and prepare a nickel salt solution for later use; (2) Preparation of reducing agent solution: Weigh 78g of sodium hydroxide and 550g of ethylene glycol, place them in a clean beaker, then add 95g of hydrazine hydrate (the hydrazine hydrate content is 60%) into the beaker, mix well, and prepare a reducing agent solution for later use; (3) First addition of reducing agent: The beaker containing the nickel salt solution in step (1) is placed in a heat-collecting constant temperature heating magnetic stirrer. Under stirring and heating, one third of the reducing agent solution in step (2) is poured into the nickel salt solution in the beaker of step (1). The pouring speed is controlled at 500 mL / min. At this time, nano nickel particles begin to form in the solution. Stirring is continued for 0.3 h. The heating temperature is 75° C. The pH value of the solution is controlled. The pH value of the solution is measured by a pH meter to be 11, thereby obtaining a solution A. (4) Second addition of reducing agent: 0.6 hours after the first addition of the reducing agent, half of the remaining reducing agent solution in step (2) was added to solution A by pouring under stirring and heating, and stirring was continued for 1.5 hours. The heating temperature was 80° C. to obtain solution B; (5) The third addition of reducing agent: 2 hours after the second addition of the reducing agent, pour all the remaining reducing agent solution in step (2) into solution B under stirring and heating, stirring for 2 hours and heating at 85°C to obtain solution C; (6) Separation of nano nickel powder: The nano nickel powder generated by the reaction is separated from solution C using a vacuum filtration device; (7) Washing and drying: The separated nano nickel powder is washed with deionized water, and then placed in a vacuum drying oven for drying, with the drying temperature controlled at 80° C., to finally obtain a nano nickel powder product.

[0024] The nano nickel powder prepared in this embodiment was subjected to SEM testing to obtain a SEM electron microscope image. Figure 2 .

[0025] Example 2 This embodiment provides a method for preparing nano nickel powder by controlled addition of a reducing agent, comprising the following steps: (1) Preparation of nickel salt solution: Weigh 155 g of nickel chloride and 1700 g of ethylene glycol, place them in a clean beaker, stir and mix them evenly, then add 35 g of PVP to the beaker to prevent the nanoparticles from agglomerating during the reaction, stir until they are completely dissolved, and prepare a nickel salt solution for later use; (2) Preparation of reducing agent solution: Weigh 78g of sodium hydroxide and 800g of ethylene glycol, place them in a clean beaker, then add 95g of hydrazine hydrate (the hydrazine hydrate content is 60%) into the beaker, mix well, and prepare a reducing agent solution for later use; (3) First addition of reducing agent: The beaker containing the nickel salt solution in step (1) is placed in a heat-collecting constant temperature heating magnetic stirrer. Under stirring and heating conditions, one third of the reducing agent solution in step (2) is poured into the nickel salt solution in the beaker of step (1). The pouring speed is controlled at 800 mL / min. At this time, nano-nickel particles begin to form in the solution. Stirring is continued for 0.4 h. The heating temperature is 75° C. and the pH of the solution is controlled to be 11. Solution A is thus obtained. (4) Second addition of reducing agent: 0.6 hours after the first addition of the reducing agent, half of the remaining reducing agent solution in step (2) was added to solution A by pouring under stirring and heating, and stirring was continued for 1.5 hours. The heating temperature was 80° C. to obtain solution B; (5) The third addition of reducing agent: 2 hours after the second addition of the reducing agent, pour all the remaining reducing agent solution in step (2) into solution B under stirring and heating, stirring for 2 hours and heating at 85°C to obtain solution C; (6) Separation of nano nickel powder: The nano nickel powder generated by the reaction is separated from solution C using a vacuum filtration device; (7) Washing and drying: The separated nano nickel powder is washed with deionized water, and then placed in a vacuum drying oven for drying, with the drying temperature controlled at 80° C., to finally obtain a nano nickel powder product.

[0026] The nano nickel powder prepared in this embodiment was subjected to SEM testing to obtain a SEM electron microscope image. Figure 3 .

[0027] Example 3 This embodiment provides a method for preparing nano nickel powder by controlled addition of a reducing agent, comprising the following steps: (1) Preparation of nickel salt solution: Weigh 165 g of nickel chloride and 2300 g of ethylene glycol, place in a clean beaker, stir and mix evenly, then add 38 g of PVP to the beaker to prevent the nanoparticles from agglomerating during the reaction, stir until completely dissolved, and prepare a nickel salt solution for later use; (2) Preparation of reducing agent solution: Weigh 64g of sodium hydroxide and 900g of ethylene glycol, place them in a clean beaker, then add 85g of hydrazine hydrate (the hydrazine hydrate content is 60%) into the beaker, mix well, and prepare a reducing agent solution for later use; (3) First addition of reducing agent: The beaker containing the nickel salt solution in step (1) is placed in a heat-collecting constant temperature heating magnetic stirrer. Under stirring and heating conditions, one third of the reducing agent solution in step (2) is poured into the nickel salt solution in the beaker of step (1). The pouring speed is controlled at 1200 mL / min. At this time, nano-nickel particles begin to form in the solution. Stirring is continued for 0.5 h. The heating temperature is 75° C. and the pH of the solution is controlled to be 11. Solution A is thus obtained. (4) Second addition of reducing agent: 0.6 hours after the first addition of the reducing agent, half of the remaining reducing agent solution in step (2) was added to solution A by pouring under stirring and heating, and stirring was continued for 1.5 hours. The heating temperature was 80° C. to obtain solution B; (5) The third addition of reducing agent: 2 hours after the second addition of the reducing agent, pour all the remaining reducing agent solution in step (2) into solution B under stirring and heating, stirring for 2 hours and heating at 85°C to obtain solution C; (6) Separation of nano nickel powder: The nano nickel powder generated by the reaction is separated from solution C using a vacuum filtration device; (7) Washing and drying: The separated nano nickel powder is washed with deionized water, and then placed in a vacuum drying oven for drying, with the drying temperature controlled at 80° C., to finally obtain a nano nickel powder product.

[0028] The nano nickel powder prepared in this embodiment was subjected to SEM testing to obtain a SEM electron microscope image. Figure 4 .

[0029] Comparative Example 1 This comparative example provides a method for preparing nano nickel powder, comprising the following steps: (1) Preparation of nickel salt solution: Weigh 155 g of nickel chloride and 1800 g of ethylene glycol, place them in a clean beaker, stir and mix them evenly, then add 32 g of PVP to the beaker to prevent the nanoparticles from agglomerating during the reaction, stir until they are completely dissolved, and prepare a nickel salt solution for later use; (2) Preparation of reducing agent solution: Weigh 64g of sodium hydroxide and 700g of ethylene glycol, place them in a clean beaker, then add 95g of hydrazine hydrate (the hydrazine hydrate content is 60%) into the beaker, mix well, and prepare a reducing agent solution for later use; (3) Adding reducing agent: The beaker containing the nickel salt solution in step (1) is placed in a heat-collecting constant temperature heating magnetic stirrer. Under stirring and heating conditions, the reducing agent solution in step (2) is poured into the nickel salt solution in the beaker in step (1) at one time. Stirring is continued for 4 hours. The heating temperature is 80° C. and the pH value of the solution is controlled to be 11. (4) Separation of nano nickel powder: Using vacuum filtration equipment to separate the nano nickel powder generated in the reaction in step (3) from the solution; (5) Washing and drying: The separated nano nickel powder is washed with deionized water, and then placed in a vacuum drying oven for drying, with the drying temperature controlled at 80° C., to finally obtain a nano nickel powder product.

[0030] The nano nickel powder prepared in this comparative example was subjected to SEM testing to obtain an SEM electron microscope image. Figure 5 .

[0031] Comparative Example 2 This comparative example provides a method for preparing nano nickel powder, comprising the following steps: (1) Preparation of nickel salt solution: Weigh 155 g of nickel chloride and 1800 g of ethylene glycol, place them in a clean beaker, stir and mix them evenly, then add 32 g of PVP to the beaker to prevent the nanoparticles from agglomerating during the reaction, stir until they are completely dissolved, and prepare a nickel salt solution for later use; (2) Preparation of reducing agent solution: Weigh 64g of sodium hydroxide and 700g of ethylene glycol, place them in a clean beaker, then add 95g of hydrazine hydrate (the hydrazine hydrate content is 60%) into the beaker, mix well, and prepare a reducing agent solution for later use; (3) First addition of reducing agent: The beaker containing the nickel salt solution in step (1) is placed in a heat-collecting constant temperature heating magnetic stirrer. Under stirring and heating conditions, half of the reducing agent solution in step (2) is poured into the nickel salt solution in the beaker of step (1). At this time, nano nickel particles begin to form in the solution. Stirring is continued for 1.5 hours. The heating temperature is 75° C. and the pH of the solution is controlled to be 11. (4) Second addition of reducing agent: 2 hours after the first addition of the reducing agent, the remaining reducing agent solution in step (2) was added to the solution in step (3) by pouring under stirring and heating, and stirring was continued for 2.5 hours. The heating temperature was 85°C; (5) Separation of nano nickel powder: Using vacuum filtration equipment to separate the nano nickel powder generated in step (4) from the solution; (6) Washing and drying: The separated nano nickel powder is washed with deionized water, and then placed in a vacuum drying oven for drying, with the drying temperature controlled at 80° C., to finally obtain a nano nickel powder product.

[0032] The nano nickel powder prepared in this comparative example was subjected to SEM testing to obtain an SEM electron microscope image. Figure 6 .

[0033] Comparative Example 3 This comparative example provides a method for preparing nano nickel powder, comprising the following steps: (1) Preparation of nickel salt solution: Weigh 155 g of nickel chloride and 1800 g of ethylene glycol, place them in a clean beaker, stir and mix them evenly, then add 32 g of PVP to the beaker to prevent the nanoparticles from agglomerating during the reaction, stir until they are completely dissolved, and prepare a nickel salt solution for later use; (2) Preparation of reducing agent solution: Weigh 64g of sodium hydroxide and 800g of ethylene glycol, place them in a clean beaker, then add 95g of hydrazine hydrate (the hydrazine hydrate content is 60%) into the beaker, mix well, and prepare a reducing agent solution for later use; (3) First addition of reducing agent: The beaker containing the nickel salt solution in step (1) is placed in a heat-collecting constant temperature heating magnetic stirrer. Under stirring and heating conditions, one quarter of the reducing agent solution in step (2) is poured into the nickel salt solution in the beaker in step (1). Stirring is continued for 0.3 h. The heating temperature is 75° C. The pH value of the solution is controlled and measured by a pH meter to be 11. (4) Second addition of reducing agent: 0.6h after the first addition of the reducing agent, one third of the remaining reducing agent solution in step (2) was added to the solution in step (3) by pouring under stirring and heating, and stirring was continued for 0.5h. The heating temperature was 75°C. (5) The third addition of reducing agent: 1.5 hours after the second addition of the reducing agent, pour half of the remaining reducing agent solution in step (2) into the solution in step (4) under stirring and heating, with a stirring time of 1.5 hours and a heating temperature of 80°C; (6) The fourth addition of reducing agent: 2 hours after the second addition of the reducing agent, pour all the remaining reducing agent solution in step (2) into the solution in step (5) under stirring and heating, with a stirring time of 2 hours and a heating temperature of 85°C; (7) Separation of nano nickel powder: Using a vacuum filtration device to separate the nano nickel powder generated by the reaction from the solution of step (6); (8) Washing and drying: The separated nano nickel powder is washed with deionized water, and then placed in a vacuum drying oven for drying, with the drying temperature controlled at 80° C., to finally obtain a nano nickel powder product.

[0034] The nano nickel powder prepared in this comparative example was subjected to SEM testing to obtain an SEM electron microscope image. Figure 7 .

[0035] Through comparative analysis Figures 2 to 7It can be seen from the electron microscope photograph that compared with adding the reducing agent once in Comparative Example 1 and adding the reducing agent twice in Comparative Example 2, the present invention controls the rate and process of the reduction reaction by gradually controlling the addition of the reducing agent three times, optimizes the nucleation and growth stages, and prevents particle agglomeration. The nano nickel powder finally obtained has a uniform particle size distribution and good dispersibility. This method simplifies the process and improves the product quality, making it of great significance in industrial production. However, compared with adding the reducing agent three times in Comparative Example 3, the particle size distribution of the nano nickel powder is not significantly improved. Considering the simplification of the process flow, improving the preparation efficiency, and reducing the production cost, it is preferred to add the reducing agent three times to achieve a uniform particle size distribution of the nano nickel powder, and prepare a nano nickel powder with excellent electrochemical properties, magnetic properties and mechanical properties to meet the application needs in the fields of electronics, energy and catalysis.

[0036] Although the preferred embodiments of the present invention have been disclosed as above, they are not intended to limit the present invention. Any person skilled in the art may make possible changes and modifications to the technical solutions of the present invention by using the methods and technical contents disclosed above without departing from the spirit and scope of the present invention. Therefore, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the contents of the technical solutions of the present invention shall fall within the protection scope of the technical solutions of the present invention.

Claims

1. A method for preparing nano nickel powder by controlled addition of a reducing agent, characterized in that: The following steps are involved: (1) Preparation of nickel salt solution: Mixing and stirring nickel salt, ethylene glycol and dispersant until they are completely dissolved to prepare a nickel salt solution; (2) Preparation of reducing agent solution: Weigh sodium hydroxide and ethylene glycol, add a reducing agent, mix well to prepare a reducing agent solution, and divide it into three equal parts by weight; (3) First addition of reducing agent: Add a portion of the reducing agent solution prepared in step (2) to the nickel salt solution prepared in step (1), keep stirring and continue heating to prepare solution A; (4) Second addition of reducing agent: Add a portion of the reducing agent solution prepared in step (2) to solution A in step (3), keep stirring and continue heating to prepare solution B; (5) Adding reducing agent for the third time: Add a portion of the reducing agent solution prepared in step (2) to solution B in step (4), keep stirring and continue heating to prepare solution C; (6) Separation of nano nickel powder: Using a vacuum filtration device to separate the nano nickel powder generated by the reaction from the solution C in step (4); (7) Washing and drying: The separated nano nickel powder is washed and then placed in a drying device for drying to finally obtain a nano nickel powder product.

2. The method for preparing nano nickel powder by controlled addition of a reducing agent according to claim 1, characterized in that: In step (1), the nickel salt solution is prepared by using 150-180 parts of nickel salt, 1500-2300 parts of ethylene glycol and 32-38 parts of dispersant, calculated by weight.

3. The method for preparing nano nickel powder by controlled addition of a reducing agent according to claim 1, characterized in that: In step (1), the nickel salt is nickel chloride, and the dispersant is polyvinyl pyrrolidone.

4. The method for preparing nano nickel powder by controlled addition of a reducing agent according to claim 1, characterized in that: In step (2), the reducing agent solution is prepared by using 60-80 parts of sodium hydroxide, 500-900 parts of ethylene glycol and 80-100 parts of reducing agent, calculated by weight.

5. The method for preparing nano nickel powder by controlled addition of a reducing agent according to claim 1, characterized in that: In step (2), the reducing agent is hydrazine hydrate.

6. The method for preparing nano nickel powder by controlled addition of a reducing agent according to claim 5, characterized in that: In step (2), hydrazine hydrate having a mass content of 60% is used.

7. The method for preparing nano nickel powder by controlled addition of a reducing agent according to claim 1, characterized in that: In the step (3), the solution stirring time is 0.3-0.5 h, the heating temperature is 75-85° C., and the pH value of the solution A is controlled at 11.

8. The method for preparing nano nickel powder by controlled addition of a reducing agent according to claim 1, characterized in that: In the step (4), the stirring time is 1-1.5 h and the heating temperature is 75-85° C.

9. The method for preparing nano nickel powder by controlled addition of a reducing agent according to claim 1, characterized in that: In the step (5), the stirring time is 1 to 3 hours and the heating temperature is 75 to 85°C.

10. The method for preparing nano nickel powder by controlled addition of a reducing agent according to claim 1, characterized in that: In step (7), the separated nano-nickel powder is washed with deionized water, and the nano-nickel powder is placed in a vacuum drying oven and dried at a drying temperature of 75-85°C.

Citation Information

Patent Citations

  • Normal-pressure production method for low-apparent-density high-purity spherical ultrafine nickel powder

    CN105081347A

  • Method for manufacturing nickel nanoparticles

    US20090025510A1

  • Nickel powder, method for manufacturing nickel powder, internal electrode paste using nickel powder, and electronic component

    US20190084040A1