Graphene composite soldering paste as well as preparation method and application thereof

By introducing graphene into the traditional Sn-Ag-Cu solder paste, forming a modified alloy solder paste and dispersing it with the FLUX solder paste, the shortcomings in mechanical strength and thermal conductivity of the traditional solder paste are solved, and the soldering is significantly improved. Reliability and quality, suitable for the high-performance welding needs of modern electronic manufacturing.

CN119035864APending Publication Date: 2024-11-29SHENZHEN AONIU TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411301430.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Traditional Sn-Ag-Cu solder paste exhibits limitations when facing the higher mechanical strength, thermal conductivity and oxidation resistance requirements in modern electronic manufacturing, making it difficult to meet miniaturization, high density and high performance electronic devices. welding requirements.

Method used

Graphene-modified Sn-Ag-Cu alloy solder paste is used to mix graphene with Sn-Ag-Cu solder paste in a specific proportion, and form alloy blocks under heating and pressure, and then spherical graphite is produced through an atomizing nozzle. The ene-Sn-Ag-Cu alloy powder and the FLUX solder paste are evenly dispersed to form a graphene composite solder paste.

Benefits of technology

It significantly improves the hardness, shear force and thermal conductivity of the solder paste, enhances the mechanical strength and heat conduction ability of the solder joints, reduces the risk of brittle failure of the solder joints, and improves the reliability and overall quality of the solder joints.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005047778080000111
    Figure BDA0005047778080000111
Patent Text Reader

Abstract

The invention discloses graphene composite soldering paste as well as a preparation method and application thereof, and graphene is added into the soldering paste, so that the performance of the soldering paste is remarkably improved. Firstly, the graphene is added, so that the hardness, shearing force and tensile strength of the soldering paste are greatly improved, a welding spot is firmer under mechanical stress, and the possibility of deformation and fracture is reduced; this enhanced mechanical strength contributes to providing a more reliable welded connection in high stress and vibration environments. And secondly, the heat-conducting property of the soldering paste is remarkably improved due to the high heat-conducting property of the graphene, so that a welding area can dissipate heat more effectively, the overheating problem is avoided, and the solder paste is particularly suitable for high-power and high-frequency electronic devices. In addition, the introduction of graphene reduces the thickness of an intermetallic compound and a bonding pad formed in the welding process, thereby not only reducing the brittleness failure risk of a welding spot, but also improving the overall quality of welding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of graphene composite solder paste, and specifically relates to a graphene composite solder paste and a preparation method and application thereof. Background Art

[0002] In the electronics manufacturing industry, solder paste is a key material in surface mount technology (SMT) and is widely used in the soldering process of printed circuit boards (PCBs). The main function of solder paste is to ensure that electronic components are reliably and firmly mounted on circuit boards by soldering the connection points between components and circuit boards. Traditional Sn-Ag-Cu (SAC305) solder paste has long been the mainstream choice for lead-free solder due to its excellent soldering performance and high fatigue resistance. However, with the continuous development of electronic devices, especially the rapid evolution towards miniaturization, high density and high performance, the physical and chemical properties of traditional solder paste have gradually failed to meet the higher requirements of modern electronic manufacturing. These changes have put forward more stringent standards for soldering materials, such as higher mechanical strength, better thermal conductivity, thinner solder joint layer and stronger anti-oxidation ability. Therefore, in the face of these new challenges, traditional SAC305 solder paste has shown some limitations and is difficult to adapt to the growing demand for soldering materials in the electronics industry.

[0003] In view of this, the present invention is proposed. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a graphene composite solder paste and a preparation method and application thereof, thereby solving the problems raised in the above-mentioned background technology.

[0005] In order to solve the above technical problems, the basic concept of the technical solution adopted by the present invention is:

[0006] A graphene composite solder paste comprises the following components in weight percentage: 0.1% to 1% graphene, 88% to 95% alloy solder paste, and 4% to 12% FLUX solder paste. The graphene-modified Sn-Ag-Cu of the present invention can improve the reliability of chips such as Fl ip~Chip IC, chip installation, PCBA, FPGA, Sip, etc. It is very important for mobile applications and vehicle applications. Compared with traditional SAC305 alloy solder paste, it has greatly improved parameters such as hardness, shear, thermal conductivity, reliability, etc., thereby achieving higher reliability.

[0007] Optionally, the alloy solder paste comprises 96.5% tin, 3.0% silver and 0.5% copper.

[0008] Optionally, the FLUX solder paste is mixed with the following ingredients: 2% to 5% of active agent, 10% to 40% of resin, 30% to 60% of isopropyl alcohol, 1% to 3% of cellulose ether, and 0.5% to 1% of benzotriazole. The water-to-binder ratio of the mixed FLUX solder paste is 1 to 2.

[0009] A method for preparing a graphene composite solder paste comprises the following steps:

[0010] Step (1), mixing graphene powder and Sn-Ag-Cu solder paste according to weight percentage, heating the mixture to 200-300° C. after mixing evenly, applying a pressure of 5-10 MPa, and maintaining it for 1-3 hours until an alloy block is formed;

[0011] Step (2), crushing the alloy block obtained in step (1) to obtain a primary powder with a particle size of 10 to 50 μm, then pouring the primary powder into a solvent, stirring it with a high-speed stirrer, and obtaining a suspension after stirring evenly;

[0012] Step (3), spraying the suspension obtained in step (2) into a drying tower at a temperature of 120 to 150° C. through an atomizing nozzle, and obtaining spherical graphene-Sn-Ag-Cu alloy powder after the droplets sprayed from the atomizing nozzle are dried;

[0013] Step (4), mixing the spherical graphene-Sn-Ag-Cu alloy powder obtained in step (3) with the flux paste in a vacuum environment until the powder and the FLUX solder paste are evenly dispersed, thereby forming a graphene composite solder paste.

[0014] Optionally, the solvent in step (2) includes but is not limited to one of ethanol, acetone or deionized water, and the weight ratio of the primary powder in step (2) to the solvent is 1:(4-10).

[0015] Optionally, a stirrer is used for stirring during the production of the suspension in step (2). The stirring speed of the stirrer during production is 1000 to 3000 rpm / min, and the stirring time is 30 to 60 min.

[0016] Optionally, in step (3), the diameter of the droplets sprayed from the atomizing nozzle is 10 to 50 um, and the spraying pressure of the atomizing nozzle is 0.1 to 0.5 MPa.

[0017] Optionally, the vacuum degree of the hollow environment in step (4) is 0.05 to 0.1 MPa, and the mixing time is 1 to 3 hours.

[0018] Optional, composite solder paste for soldering applications in mobile devices and automotive electronics.

[0019] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art. Of course, any product implementing the present invention does not necessarily need to achieve all the advantages described below at the same time:

[0020] By adding graphene to solder paste, the performance of the solder paste has been significantly improved. First, the addition of graphene greatly improves the hardness, shear force and tensile strength of the solder paste, making the solder joints more robust under mechanical stress and reducing the possibility of deformation and fracture. This enhanced mechanical strength helps to provide more reliable solder connections in high stress and vibration environments. Secondly, the high thermal conductivity of graphene significantly improves the thermal conductivity of the solder paste, allowing the soldering area to dissipate heat more effectively and avoid overheating problems, which is particularly suitable for high-power and high-frequency electronic devices. In addition, the introduction of graphene reduces the intermetallic compounds formed during the soldering process and the thickness of the pad, which not only reduces the risk of brittle failure of the solder joint, but also improves the overall quality of the soldering. DETAILED DESCRIPTION

[0021] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0022] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0023] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0024] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.

[0025] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0026] The embodiment of the present invention discloses a graphene composite solder paste, which comprises the following components in weight percentage: 0.1% to 1% of graphene, 88% to 95% of alloy solder paste, and 4% to 12% of FLUX solder paste.

[0027] In some embodiments of the present invention, the alloy solder paste comprises 96.5% tin, 3.0% silver and 0.5% copper.

[0028] A method for preparing a graphene composite solder paste comprises the following steps:

[0029] Step (1), mixing graphene powder and Sn-Ag-Cu solder paste according to weight percentage, heating the mixture to 200-300° C. after mixing evenly, applying a pressure of 5-10 MPa, and maintaining it for 1-3 hours until an alloy block is formed;

[0030] Step (2), crushing the alloy block obtained in step (1) to obtain a primary powder with a particle size of 10 to 50 μm, then pouring the primary powder into a solvent, stirring it with a high-speed stirrer, and obtaining a suspension after stirring evenly;

[0031] Step (3), spraying the suspension obtained in step (2) into a drying tower at a temperature of 120 to 150° C. through an atomizing nozzle, and obtaining spherical graphene-Sn-Ag-Cu alloy powder after the droplets sprayed from the atomizing nozzle are dried;

[0032] Step (4), mixing the spherical graphene-Sn-Ag-Cu alloy powder obtained in step (3) with the flux paste in a vacuum environment until the powder and the FLUX solder paste are evenly dispersed, thereby forming a graphene composite solder paste.

[0033] In some embodiments of the present invention, the solvent in step (2) includes but is not limited to one of ethanol, acetone or deionized water, and the weight ratio of the primary powder in step (2) to the solvent is 1:(4-10).

[0034] In some embodiments of the present invention, during the production of the suspension in step (2), a stirrer is required for stirring, and the stirring speed of the stirrer is 1000 to 3000 rpm / min and the stirring is continued for 30 to 60 min.

[0035] In some embodiments of the present invention, the diameter of the droplets sprayed from the atomizing nozzle in step (3) is 10 to 50 um, and the spraying pressure of the atomizing nozzle is 0.1 to 0.5 MPa.

[0036] In some embodiments of the present invention, the vacuum degree of the hollow environment in step (4) is 0.05-0.1 MPa, and the mixing time is 1-3 h.

[0037] The present invention will now be further described in detail with reference to embodiments.

[0038] It should be noted that all raw materials in the examples of the present invention were obtained through commercial sources.

[0039] The FLUX solder paste used in the following embodiments is mixed with the following ingredients: 5% activator, 38% resin, 55% isopropyl alcohol, 1% cellulose ether, and 1% benzotriazole. The water-to-binder ratio of the mixed FLUX solder paste is 1.2.

[0040] Embodiment 1: A method for preparing a graphene composite solder paste, comprising the following steps:

[0041] Step (1): 0.1% graphene powder and 95% Sn-Ag-Cu solder paste were mixed by weight. After uniform mixing, the mixture was placed in a hot press, heated to 250° C., and a pressure of 7 MPa was applied for 2 hours to form a dense alloy block.

[0042] Step (2): The alloy block obtained in step (1) is crushed using a mechanical crusher to obtain a primary powder with a particle size of 20 μm. The primary powder is poured into an ethanol solvent with a weight ratio of powder to solvent of 1:6. A high-speed stirrer is used to stir at a speed of 2000 rpm / min for 40 minutes to obtain a uniform suspension.

[0043] Step (3): The suspension is sprayed into a drying tower at a temperature of 130° C. through an atomizing nozzle, and the spraying pressure of the nozzle is set to 0.3 MPa. The droplets sprayed through the atomizing nozzle have a diameter of 30 μm, and the droplets evaporate rapidly in the drying tower to form spherical graphene-Sn-Ag-Cu alloy powder.

[0044] Step (4): The spherical powder obtained in step (3) is mixed with 4.9% FLUX solder paste by weight. The mixture is placed in a vacuum environment of 0.08 MPa in a vacuum mixing device and mixed for 2 hours until the powder and the solder paste are evenly dispersed, and finally a graphene composite solder paste is formed.

[0045] Embodiment 2: A method for preparing a graphene composite solder paste, comprising the following steps:

[0046] Step (1): 0.5% graphene powder and 90% Sn-Ag-Cu solder paste were mixed by weight. After uniform mixing, the mixture was placed in a hot press, heated to 220° C., and a pressure of 8 MPa was applied for 1.5 hours to form a dense alloy block.

[0047] Step (2): The alloy block obtained in step (1) is crushed using a mechanical crusher to obtain a primary powder with a particle size of 30 μm. The primary powder is poured into an acetone solvent with a weight ratio of powder to solvent of 1:8. A high-speed stirrer is used to stir at a speed of 1500 rpm / min for 50 minutes to obtain a uniform suspension.

[0048] Step (3): The suspension is sprayed into a drying tower at a temperature of 140° C. through an atomizing nozzle, and the spraying pressure of the nozzle is set to 0.2 MPa. The droplet diameter sprayed by the atomizing nozzle is 20 μm, and the droplet evaporates rapidly in the drying tower to form spherical graphene-Sn-Ag-Cu alloy powder.

[0049] Step (4): The spherical powder obtained in step (3) is mixed with 9.5% of FLUX solder paste by weight. The mixture is placed in a vacuum environment of 0.07 MPa in a vacuum mixing device and mixed for 2.5 hours until the powder and the solder paste are evenly dispersed, and finally a graphene composite solder paste is formed.

[0050] Embodiment 3: A method for preparing a graphene composite solder paste, comprising the following steps:

[0051] Step (1): 1% graphene powder and 88% Sn-Ag-Cu solder paste were mixed by weight. After uniform mixing, the mixture was placed in a hot press, heated to 300° C., and a pressure of 10 MPa was applied for 3 hours to form a dense alloy block.

[0052] Step (2): The alloy block obtained in step (1) is crushed by a mechanical crusher to obtain a primary powder with a particle size of 50 μm. The primary powder is poured into deionized water with a weight ratio of powder to solvent of 1:10. A high-speed stirrer is used to stir at a speed of 1000 rpm / min for 60 minutes to obtain a uniform suspension.

[0053] Step (3): The suspension is sprayed into a drying tower at a temperature of 150° C. through an atomizing nozzle, and the spraying pressure of the nozzle is set to 0.1 MPa. The droplets sprayed through the atomizing nozzle have a diameter of 10 μm, and the droplets evaporate rapidly in the drying tower to form spherical graphene-Sn-Ag-Cu alloy powder.

[0054] Step (4): The spherical powder obtained in step (3) is mixed with 11% FLUX solder paste by weight. The mixture is placed in a vacuum environment of 0.05 MPa in a vacuum mixing device and mixed for 3 hours until the powder and the solder paste are evenly dispersed, and finally a graphene composite solder paste is formed.

[0055] Control Example 1: A method for preparing a graphene composite solder paste, eliminating the use of graphene and retaining only alloy solder paste and FLUX solder paste, wherein the percentages of alloy solder paste and FLUX solder paste are 95% and 5%, respectively, and the other preparation methods are the same as Examples 1 to 3.

[0056] Experimental example

[0057] First, according to the preparation method in Example 1, a solder paste sample containing graphene was prepared and a traditional SAC305 alloy solder paste without graphene was prepared as a control sample.

[0058] 1. Hardness test

[0059] 1.1. Equipment: Use Vickers hardness tester (HV).

[0060] 1.2 Hardness test method:

[0061] Each solder paste sample was prepared into a specimen of standard size. Next, the specimens were placed under the hardness tester in turn and a fixed load was applied. Subsequently, the diagonal length of the indentation was recorded, the hardness value (HV) was calculated, and then each sample was measured multiple times and the average value was taken as the final hardness result. Finally, the hardness value of each sample was recorded, and the percentage of hardness improvement of the graphene composite solder paste compared to the traditional SAC305 solder paste was calculated.

[0062] 2. Shear force test

[0063] 2.2. Equipment: shear force tester.

[0064] 2.3. Shear force test method:

[0065] The solder paste samples were coated on the test substrate and solder joints were prepared according to the standard soldering process. Next, a shear force tester was used to apply lateral force to the solder joints until the solder joints broke. Subsequently, the maximum shear force value was recorded. Each solder paste sample was then tested multiple times and the average value was taken as the final shear force result. Finally, the shear force value of each sample was recorded, and the percentage increase in shear force of the graphene composite solder paste relative to the traditional SAC305 solder paste was calculated.

[0066] 3. Tensile strength test

[0067] 3.1. Equipment: tensile testing machine.

[0068] 3.2 Tensile strength test method:

[0069] The solder joints were prepared using standard methods, the solder paste samples were applied between the metal sheets, and the soldering was completed. Next, the welded metal sheets were clamped in a tensile testing machine and vertical tension was applied until the solder joint broke. Subsequently, the maximum tensile strength was recorded. Each solder paste sample was then tested multiple times and the average value was taken as the final tensile strength result. Finally, the tensile strength value of each sample was recorded, and the percentage increase in tensile strength of the graphene composite solder paste relative to the traditional SAC305 solder paste was calculated.

[0070] 4. Thermal conductivity test

[0071] 4.1. Equipment: Laser flash thermal conductivity tester.

[0072] 4.2. Thermal conductivity test method:

[0073] The solder paste samples were pressed into thin sheets. Next, the sheets were placed in a thermal conductivity tester, and laser pulses were used to generate temperature changes on the sample surface. The thermal conductivity was then calculated by measuring the time and amplitude of the temperature change. Finally, the thermal conductivity of each sample was recorded, and the percentage increase in thermal conductivity of the graphene composite solder paste compared to the traditional SAC305 solder paste was calculated.

[0074] 5. IMC thickness measurement

[0075] 5.1. Equipment: Scanning electron microscope (SEM) or optical microscope.

[0076] 5.2. IMC thickness measurement method:

[0077] Prepare the solder joint cross section, solder the solder paste sample on the substrate, cut and polish the sample to observe the solder joint cross section. Then, use a microscope to observe the IMC (intermetallic compound) layer and measure the thickness of the IMC layer. Then measure multiple samples and take the average value. Finally, record the IMC thickness of each sample and calculate the percentage reduction of IMC thickness of graphene composite solder paste relative to traditional SAC305 solder paste.

[0078] 6. Pad thickness measurement

[0079] 6.1. Equipment: optical microscope or three-dimensional microscope.

[0080] 6.2. Pad thickness measurement method:

[0081] Prepare a cross section of the solder joint, similar to the method of IMC thickness measurement. Then, use a microscope to observe the pad area of ​​the solder joint and measure the pad thickness. Finally, measure multiple samples and take the average value.

[0082] 7. Reflow soldering reliability test

[0083] 7.1. Equipment: reflow soldering furnace, microscope or X-ray inspector.

[0084] 7.2 Reflow soldering reliability test method:

[0085] The solder paste samples were coated on the printed circuit board (PCB) and components were mounted using a standard soldering process. The sample board was then soldered through a reflow soldering furnace, and reflow soldering was performed according to the specified temperature curve, with the maximum temperature set at 250°C. Subsequently, the soldered sample board was repeatedly subjected to more than 5 reflow soldering cycles in the reflow soldering furnace. After each reflow soldering, the solder joints were then inspected using a microscope or X-ray to evaluate the morphology and defects of the solder joints. Next, the solder joints were electrically tested to check electrical connectivity, and mechanical strength tests such as shear force tests and tensile tests were performed to evaluate the reliability and durability of the solder joints. Finally, the data on solder joint morphology changes, electrical connectivity, and mechanical strength changes after each reflow soldering were recorded, and the percentage of reliability improvement of the graphene composite solder paste relative to the traditional SAC305 solder paste was calculated.

[0086] 8. Results Summary

[0087] 8.1. The measurement results of hardness test, shear force test, tensile strength test, thermal conductivity test, IMC thickness measurement, pad thickness measurement, and reflow soldering reliability are shown in Table 1.

[0088] Table 1: Experimental data summary

[0089]

[0090] As shown in Table 1, compared with Example 1 and Comparative Example 1, the present invention achieves the following effects:

[0091] 1. The hardness of traditional SAC305 alloy solder paste is 15.4HV (Vickers hardness). In addition, the hardness of graphene super performance solder paste is 16.3HV, which is 0.9HV higher than that of traditional SAC305, and the hardness is increased by 5.8%. The increase in hardness shows that the addition of graphene enhances the mechanical strength of the solder paste, which helps to improve the durability and deformation resistance of the solder joints.

[0092] 2. The shear force of traditional SAC305 alloy solder paste is 200.9 grams. The shear force of graphene super performance solder paste is 208.4 grams, which is 7.5 grams more than traditional SAC305, and the shear force is increased by 4%.

[0093] The increase in shear force shows that the solder paste has a stronger shear resistance when subjected to lateral forces, which can reduce the risk of solder joints breaking during use.

[0094] 3. The tensile strength of traditional SAC305 alloy solder paste is 275.6 grams. The tensile strength of graphene super performance solder paste is 288.2 grams, which is 12.6 grams more than the traditional SAC305, and the tensile strength is increased by 4.5%. The increase in tensile strength indicates that the solder joint has a stronger ability to resist fracture when under tension, which is particularly important for welding applications that require high reliability.

[0095] 4. The thermal conductivity of traditional SAC305 alloy solder paste is 68.23W / (m·K). The thermal conductivity of graphene super performance solder paste is 84.5W / (m·K), which is 16.27W / higher than that of traditional SAC305.

[0096] (m·K), and the thermal conductivity increased by 24%. The significant improvement in thermal conductivity shows that the addition of graphene effectively improves the thermal conductivity of solder paste, which is particularly important for electronic products with strict thermal management requirements (such as high-power devices and chips), and can effectively reduce overheating problems and improve product reliability.

[0097] 5. The IMC (intermetallic compound) thickness of traditional SAC305 alloy solder paste is 4.38um. The IMC thickness of graphene super performance solder paste is 3.49um, which is 0.89um less than that of traditional SAC305, and the thickness is reduced by 25.5%. The reduction in IMC thickness helps reduce the risk of brittle failure of solder joints, because thinner IMC layers generally show higher mechanical flexibility and thermal fatigue resistance, which has an important impact on long-term reliability.

[0098] 6. The pad thickness of traditional SAC305 alloy solder paste is 3.03um. The pad thickness of graphene super performance solder paste is 2.14um, which is 0.89um less than that of traditional SAC305, and the thickness is reduced by 30%. The reduction in pad thickness further reduces the total thickness of the welding area, which helps to reduce the weight of the solder joint, improve the overall welding quality, and reduce material consumption during the welding process.

[0099] 7. By comparing the reflow soldering reliability test results of traditional SAC305 solder paste and graphene composite solder paste, it was found that the reliability of graphene composite solder paste was improved by 17% compared with traditional SAC305 solder paste after more than 5 reflow soldering cycles. This improvement shows that graphene composite solder paste has shown stronger resistance to thermal fatigue and stability during multiple reflow soldering processes, effectively reducing stress accumulation and microstructural changes in solder joints during repeated heating and cooling. This performance advantage makes graphene composite solder paste particularly suitable for the manufacture of electronic products that require high reliability and long life.

[0100] The present invention is not limited to the above-mentioned embodiments. Anyone should be aware that any structural changes made under the enlightenment of the present invention, and any technical solutions that are the same or similar to the present invention, fall within the protection scope of the present invention. The technology, shape, and structural parts not described in detail in the present invention are all well-known technologies.

Claims

1. A graphene composite solder paste, It is characterized in that The invention comprises the following components in weight percentage: 0.1% to 1% of graphene, 88% to 95% of alloy solder paste, and 4% to 12% of FLUX solder paste.

2. The graphene composite solder paste according to claim 1, It is characterized in that The alloy solder paste comprises 96.5% tin, 3.0% silver and 0.5% copper.

3. The graphene composite solder paste according to claim 1, It is characterized in that FLUX soldering paste is a mixture of the following ingredients: 2% to 5% active agent, 10% to 40% resin, 30% to 60% isopropyl alcohol, 1% to 3% cellulose ether, and 0.5% to 1% benzotriazole. The water-to-gel ratio of the mixed FLUX soldering paste is 1 to 2.

4. A method for preparing a graphene composite solder paste, It is characterized in that The following steps are involved: Step (1), mixing graphene powder and Sn-Ag-Cu solder paste according to weight percentage, heating the mixture to 200-300° C. after mixing evenly, applying a pressure of 5-10 MPa, and maintaining it for 1-3 hours until an alloy block is formed; Step (2), crushing the alloy block obtained in step (1) to obtain a primary powder with a particle size of 10 to 50 μm, then pouring the primary powder into a solvent, stirring with a stirrer, and obtaining a suspension after stirring evenly; Step (3), spraying the suspension obtained in step (2) into a drying tower at a temperature of 120 to 150° C. through an atomizing nozzle, and obtaining spherical graphene-Sn-Ag-Cu alloy powder after the droplets sprayed from the atomizing nozzle are dried; Step (4), mixing the spherical graphene-Sn-Ag-Cu alloy powder obtained in step (3) with the flux paste in a vacuum environment until the powder and the FLUX solder paste are evenly dispersed, thereby forming a graphene composite solder paste.

5. A method for preparing a graphene composite solder paste according to claim 4, It is characterized in that The solvent in step (2) includes but is not limited to one of ethanol, acetone or deionized water, and the weight ratio of the primary powder in step (2) to the solvent is 1:(4-10).

6. A method for preparing a graphene composite solder paste according to claim 4, It is characterized in that During the production of the suspension in step (2), a stirrer is required for stirring. During production, the stirring speed of the stirrer is 1000 to 3000 rpm / min, and the stirring time is 30 to 60 min.

7. A method for preparing a graphene composite solder paste according to claim 4, It is characterized in that In step (3), the diameter of the droplets sprayed from the atomizing nozzle is 10 to 50 μm, and the spraying pressure of the atomizing nozzle is 0.1 to 0.5 MPa.

8. A method for preparing a graphene composite solder paste according to claim 4, It is characterized in that The vacuum degree of the hollow environment in step (4) is 0.05-0.1 MPa, and the mixing time is 1-3 hours.

9. An application of the graphene composite solder paste according to any one of claims 1 to 3 in welding of mobile devices and vehicle-mounted electronic devices.