Main shaft welding repair process
By performing welding repair on the main shaft of the exhaust gas recovery turbine power generation unit, the problem of main shaft cracking was solved, the cost and cycle were reduced, the welding performance and manufacturing precision were improved, and the high strength and high toughness requirements of martensitic stainless steel materials were met.
Patent Information
- Application Number
- CN202411192355.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-29
AI Technical Summary
In existing technologies, the main shaft of the exhaust gas recovery turbine power generation device needs to be repaired by integral forging due to cracking, resulting in high costs and long cycles. Furthermore, the martensitic stainless steel material has poor weldability, posing unknown risks and making it difficult to meet the requirements of high strength and high toughness.
The welding repair process is carried out on the repair shaft. The new shaft head is made by interference fit, preheating, positioning welding, multi-layer and multi-pass welding, and post-weld stress relief treatment to ensure the strength and accuracy of the weld. Special welding materials and welding parameters are used, and deformation is monitored and the welding direction is adjusted.
This reduces spindle manufacturing costs and cycle time, improves welding performance, meets the high strength and high toughness requirements of martensitic stainless steel materials, and ensures spindle manufacturing accuracy and safety.
Smart Images

Figure CN119035984A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of spindle repair, in particular to a spindle welding repair process. Background Art
[0002] The exhaust gas recovery turbine power generation device is a secondary energy recovery device that can convert the internal energy of the high-temperature and high-pressure exhaust gas generated by the industrial production line into mechanical energy or electrical energy, thereby realizing energy recycling.
[0003] The main shaft is the core component of the exhaust gas recovery turbine power generation device. The main shaft is made of martensitic stainless steel material and processed after integral forging. Due to the harsh operating conditions, some units in the exhaust gas recovery turbine power generation device were found to have cracks in the shaft head part of the main shaft during the maintenance process, which brought great hidden dangers to the safe operation of the unit and the entire production line. At present, the solution of remaking the entire forging is adopted for repair. However, the main shaft is made of martensitic stainless steel material for integral forging, which has high manufacturing cost and brings great economic losses to users. The shutdown of the exhaust gas recovery turbine power generation device will affect the energy recovery of the production line, causing huge waste and environmental pollution. Therefore, if the defective part of the main shaft (i.e. the repair shaft) can be removed and a new shaft head can be made to repair the main shaft to form a new main shaft, the manufacturing cost and cycle can be greatly reduced.
[0004] However, because the spindle is made of martensitic stainless steel, the material has poor weldability, and there are unknown risks in the welding, post-welding and subsequent operation of the spindle, so the spindle repair weld must meet the high strength requirements of martensitic stainless steel. In addition, the spindle manufacturing has high precision requirements, and the spindle end and key parts need to meet the spindle runout value ≤ 0.02mm to ensure that the spindle accuracy meets the requirements after welding repair. Therefore, it is very necessary to design a spindle welding repair process that can repair the spindle on the original spindle repair shaft. Summary of the invention
[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a spindle welding repair process, which, by performing repairs on the original spindle, not only greatly reduces the manufacturing cost and cycle of the spindle, but also improves the welding performance of the material, so that the spindle repair weld can meet the high strength and high toughness requirements of martensitic stainless steel materials. At the same time, the spindle manufacturing accuracy is guaranteed by monitoring the runout value of the spindle shaft end and adjusting the welding direction according to the runout value.
[0006] In order to solve the above technical problems, the present invention provides a spindle welding repair process, through which a new spindle head and a repaired spindle are assembled into one body to form a new spindle, and the welding repair process includes the following steps:
[0007] A new shaft head is installed on the bearing of the repaired shaft by interference heat treatment. A groove weld is provided on the new shaft head, and the interference between the new shaft head and the repaired shaft is 0.38 mm to 0.48 mm.
[0008] The new shaft head and the repaired shaft after hot-loading need to be preheated before welding. The preheating area is the connection area between the new shaft head and the repaired shaft including the groove weld. The cross-sectional length of the preheating area is 200mm to 1m, and it avoids the blade root groove position of the repaired shaft. When the preheating area is heated, in order to facilitate timely monitoring of the deformation of the repaired shaft, the repaired shaft needs to be rotated;
[0009] After preheating, the repaired shaft and shaft head need to be welded. When welding, first perform positioning welding along the bottom of the groove weld. When positioning welding, four points need to be evenly distributed. The four-point positioning welding is symmetrical. The length of the positioning welding is 10mm to 20mm. Then, the groove weld is welded by multi-layer and multi-pass welding. The first to second base layers, filling layers and cover layers are welded. When welding the filling layer and the cover layer, the welding needs to be symmetrical. The diameter of the welding rod used for the first to second base layers is smaller than that used for the filling layer and the cover layer. During the welding process, the interlayer temperature of the first to second base layers, the filling layer and the cover layer cannot exceed 350℃.
[0010] Monitor the deformation of the shaft end of the repaired shaft from the welding of the second base layer. When the deformation of the shaft end of the repaired shaft exceeds 0.02mm, welding is required at the reverse position of the deformation of the repaired shaft.
[0011] After welding, the repaired shaft needs to be stress relieved by rotating and heating.
[0012] Preferably, the preheating temperature is 250°C to 350°C, the preheating time is 5h to 8h, the preheating temperature rise rate is ≤100°C / h, and the repair shaft rotation speed is 0.05r / min to 0.3r / min.
[0013] Preferably, the first and second base layers are welded using electrodes with a diameter of 3.2 mm, and the filling layer and the cover layer are welded using electrodes with a diameter of 4.0 mm; the welding conditions are as follows:
[0014] The welding current of the 3.2mm diameter electrode is 70A~120A, the arc voltage is 22V~26V, and the welding speed is 17cm / min~25cm / min;
[0015] The welding current of the 4.0mm diameter electrode is 90A~150A, the arc voltage is 22V~26V, and the welding speed is 19cm / min~30cm / min.
[0016] Preferably, the repaired shaft is rotated and placed in a local rotation preheating stress relief furnace to relieve the stress of the repaired shaft, wherein the stress relief processing parameters of the repaired shaft are: the temperature rise of the local rotation preheating stress relief furnace is ≤50°C / h, when the furnace temperature of the local rotation preheating stress relief furnace is 420°C, the repaired shaft is relieved of stress at 420°C, and the stress relief insulation time is 4h to 6h , The repaired shaft is kept warm and then furnace cooled. When the temperature of the local rotary preheating and stress relief furnace is lower than 250°C, the repaired shaft is removed from the local rotary preheating and stress relief furnace.
[0017] Preferably, the hot installation is performed by uniformly heating the new shaft head with an oxyacetylene flame in the hot installation well, and after preheating, the groove weld connecting the new shaft head and the repaired shaft area is covered with a heat insulating material for insulation.
[0018] Preferably, before preheating the welding part of the newly manufactured shaft head, pre-welding preparation is required, including the following steps:
[0019] (1) The welding rod pretreatment needs to be baked at 300℃~400℃ for 1h~2h and then stored in a constant temperature insulation barrel;
[0020] (2) Determine the polarity of the welding power supply. The connection method between the welding power supply and the first to second base layers, filling layers, and cover layers should all adopt the DC reverse connection method;
[0021] (3) Before welding, clean the impurities in the groove weld of the newly made shaft head so that the surface of the groove weld reveals the metallic luster.
[0022] Preferably, a reference surface is set on the repair shaft near the groove weld. The reference surface of the repair shaft needs to be bright-processed before welding. The axial width of the reference surface is 20 mm, and the diameter of the reference surface of the repair shaft needs to be similar to the diameter at the weld.
[0023] Preferably, after welding, the welding part needs to be cleaned, the welding area needs to be polished, and a penetrant inspection needs to be performed.
[0024] Preferably, after welding, the repair shaft needs to be aligned according to the reserved reference surface and the journal of the repair shaft, and the new shaft head and journal need to be machined, with the journal runout value ≤0.02mm. After the journals on both sides are machined, the journals on both sides are converted to the machining reference, and then the new shaft head and welded joint are finished.
[0025] Preferably, a margin of 0.5 mm to 1 mm is reserved for non-destructive testing of the weld joint.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1. The present invention forms a firm connection between the new shaft head and the repaired shaft by interference fit, which can effectively transfer load and prevent slippage, thereby ensuring the overall strength. The present invention preheats the new shaft head and the repaired shaft after hot-fitting before welding, which can reduce the cooling rate of the welding molten pool, avoid the generation of hardened structure, avoid weld cracking, and further improve the strength of the main shaft repair weld. During welding, the groove weld is welded by a multi-layer multi-pass welding method for the first to second base layers, filling layers and cover layers. When welding the filling layer and the cover layer, symmetrical welding is required. The diameter of the welding rod used in the first to second base layers is smaller than the diameter of the welding rod used in the filling layer and the cover layer, which can ensure the optimal welding performance of the root weld and ensure the welding quality. During the welding process, the welding current and voltage of the first to second base layers, filling layers and cover layers cannot exceed 150A, and the interlayer temperature cannot exceed 350℃. The two welding methods are combined to meet the high strength requirements of welds of dissimilar materials. In addition, after welding, the repaired shaft is heated by rotation to eliminate stress, thereby avoiding cracking of the weld due to the formation of brittle structure in the middle part of the weld of the new main shaft, thereby meeting the high strength requirements of welds of dissimilar materials.
[0028] The present invention reduces the matching clearance and improves the overall accuracy by hot-fitting the new shaft head onto the repair shaft through interference fit, and then the new shaft head and the repair shaft are closely matched. In addition, the interference fit can ensure the stable and close connection between the shaft head and the repair shaft, thereby reducing the operation error caused by poor matching. In addition, during preheating, the deformation of the repair shaft can be timely monitored by rotating the repair shaft, which is convenient for real-time monitoring of the manufacturing accuracy of the main shaft. After preheating, the repair shaft and the shaft head are welded. When welding, positioning welding is first performed along the bottom of the groove weld. When positioning welding, four-point positioning is evenly distributed, and four-point positioning is symmetrically welded (that is, two people weld symmetrically at the same time, and then rotate 90° and weld symmetrically again at the same time). The purpose of this is to control the cocenter of the new shaft head and the repair shaft, so as to ensure the manufacturing accuracy of the main shaft. In addition, the deformation of the shaft end of the repaired shaft is monitored starting from the welding of the second base layer. When the deformation of the shaft end of the repaired shaft exceeds 0.02mm, it is necessary to weld the repaired shaft in the reverse position and rotate and heat the repaired shaft after welding to eliminate stress. Both can ensure the welding accuracy of the main shaft. This is because the strength of the repaired main shaft increases after welding. In this process, the deformation of the repaired shaft is difficult to adjust. Therefore, it is necessary to ensure that the new shaft head is concentric with the repaired shaft on the basis of strength assurance. The repair process monitors the deformation of the shaft end of the repaired shaft from the second layer to ensure the manufacturing accuracy of the main shaft.
[0029] 2. The welding repair process provided by the present invention can greatly shorten the repair cycle. This is because there are few manufacturers with the ability to forge large stainless steel forgings, and the manufacturing cycle is long. If only an alloy steel shaft head is to be repaired, there are many forging manufacturers, the cycle is very short, and the shaft repair cycle is also short.
[0030] 3. The repair cost of the welding repair process provided by the present invention is very low. This is because the new shaft head is made of alloy steel forgings, and the forging cost is low. Compared with the new main shaft, the cost is greatly reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The present invention is a main shaft welding repair process diagram.
[0032] Figure 2 It is a repair shaft diagram in a main shaft welding repair process of the present invention.
[0033] Figure 3 It is a partial view of the shaft head and the repair shaft in a main shaft welding repair process of the present invention.
[0034] Figure 4 The present invention is a main shaft welding repair process for the main shaft and the new shaft head in the integrated assembly process using the welding repair process.
[0035] Figure Annotation
[0036] 1. Blade root groove, 2. Groove weld, 3. Bearing, 4. Main shaft, 5. New shaft head, 6. Reference surface, 7. Heating area, 8. Support area. DETAILED DESCRIPTION
[0037] In order to make the above-mentioned purposes, features and advantages of the embodiments of the present invention more obvious and understandable, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention. All other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] The inventor found that the cracked spindle head is currently repaired by remaking the entire forging. However, resetting the entire forging not only increases the cost, but also causes the unit to shut down, affecting the energy recovery of the production line. This is because the spindle forging is relatively large, and only a few forging manufacturers can make it, and the manufacturing cycle is very long. In addition, the spindle forging is a large stainless steel forging, and the cost of making a new one is high. Therefore, the inventor found that if the newly made shaft head can be repaired on the original repair shaft, only one shaft head needs to be remade, which can greatly reduce the manufacturing cost and cycle. Therefore, the idea of repairing on the original spindle is proposed, but due to the poor weldability of the high-alloy steel spindle, there are unknown risks in the spindle during welding, post-welding and subsequent operation. Therefore, which welding repair process can meet the user's use requirements, can improve the spindle manufacturing accuracy, and can also make the runout value of the spindle shaft end and key parts meet the requirement of ≤0.02mm. This is the key to the welding repair process, so that the spindle repair weld can meet the high strength and high toughness requirements of martensitic stainless steel materials.
[0039] In view of this, the present invention greatly reduces the manufacturing cost and cycle of the new main shaft by performing repair on the repair shaft.
[0040] like Figure 1 As shown, the present invention provides a structural schematic diagram of the main shaft 4 and the newly manufactured shaft head 5 and a structural schematic diagram of the main shaft and the newly manufactured shaft head being integrated into one by a welding repair process.
[0041] like Figure 1-2 As shown, the main shaft 4 is provided with a plurality of blade root grooves 1 around the circumference, and the blade root grooves 1 arranged on the cross section of the main shaft 4 are symmetrically arranged in pairs along the horizontal axis. A new shaft head 5 is heat-installed on the left end of the main shaft 4, and a groove weld 2 is provided on the new shaft head 5 close to the blade root groove 1. Two bearings 3 are respectively on the groove weld away from the new shaft head 5 and on the main shaft 4 away from the blade root groove 1.
[0042] like Figure 3-4 As shown, before the main shaft 4 and the new shaft head 5 are integrated into an integrated structure by welding repair process, support areas 8 need to be set on the main shaft 4 and the new shaft head 5 respectively, for installing the support components at the support areas 8, so as to facilitate the subsequent assembly process. The support area 8 on the new shaft head 5 is set between the bearing 3 and the groove weld 2 of the new shaft head 5; the support area 8 on the main shaft 4 is set between the blade root groove 1 and the bearing 3. The heating area 7 is located in the groove weld area including the groove weld connecting the new shaft head and the repaired shaft.
[0043] The welding repair process for the new shaft head and the repaired shaft provided in the present invention ensures the manufacturing strength requirements of the main shaft. The welding repair process used in the present invention is to achieve the same weld strength as the original main shaft base material strength through interference fit of the new shaft head and the repaired shaft, preheating of the repaired shaft, welding of the repaired shaft and the new main shaft, and control of welding parameters and repaired shaft stress relief process, thereby meeting the design requirements and avoiding cracking during subsequent main shaft operation. The repair scheme has been verified by multiple products.
[0044] The welding repair process of the new shaft head and the repair shaft provided by the present invention ensures that the welding deformation of the main shaft manufacturing meets the requirements. During the welding repair process, the deformation of the shaft end of the repair shaft is monitored by local rotation preheating, positioning welding, positioning welding parameter control, and the second base layer. Then, by monitoring the runout value of the main shaft end and adjusting the welding direction according to the runout value, the deformation accuracy of the shaft ends on both sides after repair is ensured to be ≤0.02mm, thereby ensuring the manufacturing accuracy of the main shaft and thus ensuring that the accuracy of the main shaft size after welding repair meets the requirements.
[0045] The present invention provides a spindle welding repair process, through which a new spindle head and a repaired spindle are assembled into one body to form a new spindle, and the welding repair process comprises the following steps:
[0046] A new shaft head is installed on the bearing of the repaired shaft by interference heat treatment. A groove weld is provided on the new shaft head, and the interference between the new shaft head and the repaired shaft is 0.38 mm to 0.48 mm.
[0047] The new shaft head and the repaired shaft after hot-loading need to be preheated before welding. The preheating area is the connection area between the new shaft head and the repaired shaft including the groove weld. The cross-sectional length of the preheating area is 200mm to 1m, and it avoids the blade root groove position of the repaired shaft. When the preheating area is heated, in order to facilitate timely monitoring of the deformation of the repaired shaft, the repaired shaft needs to be rotated;
[0048] After the preheating is completed, the repair shaft and the shaft head need to be welded. When welding, tack welding is first performed along the bottom of the groove weld. When tack welding, four points need to be evenly distributed for positioning. The four-point positioning is symmetrically welded, and the tack welding length is 10mm-20mm; then the groove weld is welded with the first to second base layers, the filling layer and the cover layer by a multi-layer and multi-pass welding method. When welding the filling layer and the cover layer, symmetric welding is required. The diameter of the welding rod used in the first to second base layers is smaller than the diameter of the welding rod used in the filling layer and the cover layer. During the welding process, the interlayer temperature of the first to second base layers, the filling layer and the cover layer cannot exceed 350°C; the welding rod used in the present invention is a special repair welding material of our company, which contains Ni (8.5%-10%), Cr (28%-33%), and Mn (1%-2.5%) elements in suitable proportions. In addition, the groove weld composition opened by the newly made shaft head is austenite, containing delta ferrite strengthening phase, so that the welded joint has high strength.
[0049] Monitor the deformation of the shaft end of the repaired shaft from the welding of the second base layer. When the deformation of the shaft end of the repaired shaft exceeds 0.02mm, welding is required at the reverse position of the deformation of the repaired shaft.
[0050] After welding, the repaired shaft needs to be stress relieved by rotating and heating.
[0051] Specifically, the preheating temperature is 250℃~350℃, the preheating time is 5h~8h, the preheating temperature rise rate is ≤100℃ / h, and the repair shaft rotation speed is 0.05r / min~0.3r / min. The preheating temperature, preheating time and preheating temperature rise rate are designed to ensure the optimal welding state and facilitate welding quality assurance. The repair shaft rotation speed can be adjusted according to the change of shaft diameter.
[0052] Specifically, the first and second base layers are welded using a welding rod with a diameter of 3.2 mm, and the filling layer and the cover layer are welded using a welding rod with a diameter of 4.0 mm; the welding conditions during welding are as follows:
[0053] The welding current of the 3.2mm diameter electrode is 70A~120A, the arc voltage is 22V~26V, and the welding speed is 17cm / min~25cm / min;
[0054] The welding current of the 4.0mm diameter electrode is 90A~150A, the arc voltage is 22V~26V, and the welding speed is 19cm / min~30cm / min.
[0055] The first and second base layers are welded with electrodes having a diameter of 3.2 mm, and the filling layer and the cover layer are welded with electrodes having a diameter of 4.0 mm, in order to better match the groove weld.
[0056] The welding conditions of 3.2mm diameter electrodes and 4.0mm diameter electrodes are set to match the welding operation performance. When the welding current of 3.2mm diameter electrodes is higher than 120A, the weld performance will be affected. When the welding current of 3.2mm diameter electrodes is lower than 70A, welding defects are likely to occur. When the welding current of 4.0mm diameter electrodes is higher than 150A, the weld performance will be affected. When the welding current of 4.0mm diameter electrodes is lower than 90A, welding defects are likely to occur.
[0057] Specifically, the repaired shaft is rotated and placed in a local rotation preheating stress relief furnace to relieve the stress of the repaired shaft. The stress relief processing parameters of the repaired shaft are: the temperature rise of the local rotation preheating stress relief furnace is ≤50℃ / h. When the furnace temperature of the local rotation preheating stress relief furnace is 420℃, the repaired shaft is stress relieved at 420℃, and the stress relief insulation time is 4h to 6h. , The repaired shaft is kept warm and then furnace cooled. When the temperature of the local rotary preheating and stress relief furnace is lower than 250°C, the repaired shaft is removed from the local rotary preheating and stress relief furnace.
[0058] There are two reasons for performing rotary preheating to relieve stress: (1) Due to the spindle welding process, high temperature weld joints are prone to produce brittle structures, which affects weld performance, while low temperature affects weld stress removal; (2) The spindle has high precision. High temperature increases the risk of deformation and causes surface oxidation, which is not conducive to precision assurance.
[0059] Specifically, during hot installation, the new shaft head is evenly heated with an oxyacetylene flame in a hot installation well, and after preheating, the groove weld connecting the new shaft head and the repaired shaft area is covered with a heat insulating material for insulation.
[0060] Specifically, before preheating the welding part of the newly manufactured shaft head, pre-welding preparation is required, including the following steps:
[0061] (1) The welding rod pretreatment needs to be baked at 300℃~400℃ for 1h~2h and then stored in a constant temperature insulation barrel. The purpose is to remove moisture from the welding rod, which is beneficial to ensure the welding performance of the welding rod;
[0062] (2) Determine the polarity of the welding power supply. The connection method between the welding power supply and the first to second base layers, filling layers, and cover layers should all adopt the DC reverse connection method;
[0063] (3) Before welding, clean the impurities in the groove weld of the newly made shaft head so that the metal luster is exposed on the surface of the groove weld, ensuring that no harmful impurities enter the weld, which is beneficial to ensure the welding performance of the electrode.
[0064] Specifically, a reference surface is set on the repair shaft near the groove weld. The reference surface of the repair shaft needs to be bright processed before welding. The axial width of the reference surface is 20 mm. The diameter of the reference surface position of the repair shaft and the diameter at the weld need to be similar. The diameter of the reference surface position of the repair shaft and the diameter at the weld need to be similar here to meet the sensitivity of alignment.
[0065] Specifically, after welding, it is necessary to clean the welding area, grind the welding area, and perform penetrant testing.
[0066] Specifically, after the repair shaft is welded, it is necessary to align it according to the reserved reference surface and the journal of the repair shaft, and process the new shaft head and journal. The journal runout value is ≤0.02mm. After the journals on both sides are processed, the journals on both sides are converted into processing references, and then the new shaft head and welded joint are finished.
[0067] Specifically, a margin of 0.5 mm to 1 mm is reserved for non-destructive testing of the weld joint.
[0068] The technical solution of the present invention is further illustrated below in the form of specific examples.
[0069] Example 1
[0070] (1) Pre-welding processing requirements:
[0071] Repair shaft reference surface: A reference surface is set on the repair shaft near the groove weld. The repair shaft reference surface needs to be bright processed before welding. The axial width of the reference surface is 20mm, and the diameter of the repair shaft reference surface position must be close to the diameter at the weld.
[0072] A new shaft head is fitted onto the bearing of the repaired shaft by interference fit, the interference between the new shaft head and the bearing of the repaired shaft is 0.40 mm, and a groove weld is provided on the new shaft head.
[0073] Use oxyacetylene flame to evenly heat the new shaft head in the hot-fitting well, and hot-fit the new shaft head onto the repaired shaft.
[0074] (2) Preparation before welding:
[0075] The welding rods used are special repair welding rods with a diameter of 3.2mm and 4mm. The welding rods need to be baked at 350℃ for 2h before welding and then stored at a constant temperature and can be taken out when needed.
[0076] Make sure the polarity of the welding power supply and the connection method of the welding power supply are DC reverse connection;
[0077] Before welding, clean the impurities in the groove weld of the newly made shaft head to make the surface of the groove weld show metallic luster;
[0078] (3) Preheating
[0079] The preheating area is the connection area between the new shaft head and the repair shaft, including the groove weld. The cross-sectional length of the preheating area is 200 mm, and it avoids the blade root groove position of the repair shaft. When the preheating area is heated, the repair shaft needs to be rotated in order to facilitate timely monitoring of the deformation of the repair shaft.
[0080] The repaired shaft and the newly manufactured shaft head should be machined away from the bearing and preheating area, and supported by supports; the repaired shaft should be rotated during heating in the preheating area to facilitate timely monitoring of the repaired shaft deformation; heat treatment parameters during preheating: temperature rise ≤50℃ / h, preheat at 300℃ for 6h; the repaired shaft rotates while heating, with a speed of 0.2r / min. After preheating, the furnace body needs to be removed, and the surrounding area of the weld should be covered with insulation materials for insulation.
[0081] (4) Welding
[0082] When welding, first perform positioning welding along the bottom of the groove weld. When positioning welding, four points must be evenly distributed, and the four-point positioning welding is symmetrical, and the welding length is 10mm. Then use the multi-layer and multi-pass welding method to weld the first to second base layers, filling layers and cover layers of the groove weld. When welding the filling layer and the cover layer, the welding must be symmetrical. The diameter of the welding rod used for the first to second base layers is smaller than the diameter of the welding rod used for the filling layer and the cover layer. During the welding process, the interlayer temperature of the first to second base layers, the filling layer and the cover layer is 300℃.
[0083] The welding parameters are as follows: the first and second base layers use 3.2mm diameter electrodes, the remaining filling layers and cover layers use 4mm diameter electrodes, and low current is required for welding. The interlayer temperature between layers cannot exceed 350℃. The welding parameters are as follows:
[0084] 3.2mm diameter welding rod: welding current is 105A, arc voltage is 22V-24V, welding speed is 20cm / min.
[0085] 4.0mm diameter welding rod: welding current is 145A, arc voltage is 22V-24V, welding speed is 28cm / min.
[0086] Beginning from welding the second base layer, monitor the deformation of the repaired shaft end. When the deformation runout of the repaired shaft end does not exceed 0.02mm, perform welding evenly and symmetrically.
[0087] (4) After welding, the repaired shaft needs to be heated by rotation to eliminate stress.
[0088] (5) The repaired shaft is rotated and placed in a local rotating preheating stress relief furnace to relieve the stress of the repaired shaft. The stress relief processing parameters of the repaired shaft are: the temperature rise of the local rotating preheating stress relief furnace is 50°C / h. When the furnace temperature of the local rotating preheating stress relief furnace is 420°C, the repaired shaft is stress relieved at 420°C, and the stress relief insulation time is 4h. , The repaired shaft is kept warm and then furnace cooled. When the temperature of the local rotary preheating and stress relief furnace is lower than 250°C, the repaired shaft is removed from the local rotary preheating and stress relief furnace.
[0089] (6) NDT: Clean the welding parts, polish them, and perform penetrant testing according to the drawing requirements.
[0090] (7) Post-weld processing:
[0091] After the repair shaft is welded, it is necessary to align the reserved reference surface and the journal of the repair shaft, and process the new shaft head journal. The runout value of the repair shaft is 0.01mm. After the journals on both sides are processed, the journals on both sides are converted to the processing reference, and then the new shaft head and the welded joint are finished. Reserve 1mm margin for non-destructive testing of the new shaft head, and after passing the test, it will be finished to meet the drawing requirements.
[0092] Example 2
[0093] 1) Pre-welding processing requirements:
[0094] Repair shaft reference surface: A reference surface is set on the repair shaft near the groove weld. The repair shaft reference surface needs to be bright processed before welding. The axial width of the reference surface is 20mm, and the diameter of the repair shaft reference surface position must be close to the diameter at the weld.
[0095] A new shaft head is fitted onto the bearing of the repaired shaft by interference fit, the interference between the new shaft head and the bearing of the repaired shaft is 0.42mm, and a groove weld is provided on the new shaft head.
[0096] Use oxyacetylene flame to evenly heat the new shaft head in the hot-fitting well, and hot-fit the new shaft head onto the repaired shaft.
[0097] (2) Preparation before welding:
[0098] The welding rods used are special repair welding rods with a diameter of 3.2mm and 4mm. The welding rods need to be baked at 350℃ for 2h before welding and then stored at a constant temperature and can be taken out when needed.
[0099] Make sure the polarity of the welding power supply and the connection method of the welding power supply are DC reverse connection;
[0100] Before welding, clean the impurities in the groove weld of the newly made shaft head to make the surface of the groove weld show metallic luster;
[0101] (3) Preheating
[0102] The preheating area is the connection area between the new shaft head and the repair shaft, including the groove weld. The cross-sectional length of the preheating area is 800mm, and it avoids the blade root groove position of the repair shaft. When the preheating area is heated, in order to facilitate timely monitoring of the deformation of the repair shaft, the repair shaft needs to be rotated;
[0103] The repaired shaft and the newly manufactured shaft head should be machined away from the bearing and preheating area and supported by supports; the repaired shaft should be rotated during heating in the preheating area to facilitate timely monitoring of the repaired shaft deformation; the heat treatment parameters during preheating are: temperature rise 90℃ / h, preheating at 350℃ for 6h; the repaired shaft rotates while heating, with a speed of 0.18r / min. After preheating, the furnace body needs to be removed, and the surrounding area of the weld should be covered with insulation materials for insulation.
[0104] (4) Welding
[0105] When welding, first perform positioning welding along the bottom of the groove weld. When positioning welding, four points must be evenly distributed, and the four-point positioning welding is symmetrical, with a welding length of 15mm. Then use the multi-layer and multi-pass welding method to weld the first to second base layers, filling layers and cover layers of the groove weld. When welding the filling layer and the cover layer, the welding must be symmetrical. The diameter of the welding rod used for the first to second base layers is smaller than that used for the filling layer and the cover layer. During the welding process, the interlayer temperature of the first to second base layers, the filling layer and the cover layer cannot exceed 350℃.
[0106] The welding parameters are as follows: the first and second base layers use 3.2mm diameter electrodes, the remaining filling layers and cover layers use 4mm diameter electrodes, and low current is required for welding. The interlayer temperature between layers cannot exceed 350℃. The welding parameters are as follows:
[0107] 3.2mm diameter welding rod: welding current is 100A, arc voltage is 22V-25V, welding speed is 23cm / min.
[0108] 4.0mm diameter welding rod: welding current is 145A, arc voltage is 22V-24V, welding speed is 27cm / min.
[0109] The deformation of the shaft end of the repaired shaft was monitored starting from the welding of the second base layer. When welding the third layer, it was found that the deformation of the shaft end of the repaired shaft exceeded 0.02mm. After two welding passes in the reverse position, the deformation jumped by 0.08. Then, welding was continued according to the original process parameters.
[0110] (6) After welding, the repaired shaft needs to be stress-eliminated by rotating heating.
[0111] (7) The repaired shaft is rotated and placed in a local rotating preheating stress relief furnace to relieve the stress of the repaired shaft. The stress relief processing parameters of the repaired shaft are: the temperature rise of the local rotating preheating stress relief furnace is 50°C / h. When the furnace temperature of the local rotating preheating stress relief furnace is 420°C, the repaired shaft is relieved of stress at 420°C, and the stress relief insulation time is 6 hours. , The repaired shaft is kept warm and then furnace cooled. When the temperature of the local rotary preheating and stress relief furnace is lower than 250°C, the repaired shaft is removed from the local rotary preheating and stress relief furnace.
[0112] (6) NDT: Clean the welding parts, polish them, and perform penetrant testing according to the drawing requirements.
[0113] (7) Post-weld processing:
[0114] After the repair shaft is welded, it is necessary to align the reserved reference surface and the journal of the repair shaft, and process the new shaft head journal. The runout value of the repair shaft is 0.013mm. After the journals on both sides are processed, the journals on both sides are converted to the processing reference, and then the new shaft head and welded joint are finished. 1mm margin is reserved for non-destructive testing of the new shaft head, and after passing the test, it is turned to finish processing to meet the requirements of the drawing.
[0115] Example 3
[0116] 1) Pre-welding processing requirements:
[0117] Repair shaft reference surface: A reference surface is set on the repair shaft near the groove weld. The repair shaft reference surface needs to be bright processed before welding. The axial width of the reference surface is 1m, and the diameter of the repair shaft reference surface position must be close to the diameter at the weld.
[0118] A new shaft head is fitted onto the bearing of the repaired shaft by interference fit, the interference between the new shaft head and the bearing of the repaired shaft is 0.44mm, and a groove weld is provided on the new shaft head.
[0119] Use oxyacetylene flame to evenly heat the new shaft head in the hot-fitting well, and hot-fit the new shaft head onto the repaired shaft.
[0120] (2) Preparation before welding:
[0121] The welding rods used are special repair welding rods with a diameter of 3.2mm and 4mm. The welding rods need to be baked at 350℃ for 2h before welding and then stored at a constant temperature and can be taken out when needed.
[0122] Make sure the polarity of the welding power supply and the connection method of the welding power supply are DC reverse connection;
[0123] Before welding, clean the impurities in the groove weld of the newly made shaft head to make the surface of the groove weld show metallic luster;
[0124] (3) Preheating
[0125] The preheating area is the connection area between the new shaft head and the repair shaft, including the groove weld. The cross-sectional length of the preheating area is 200 mm, and it avoids the blade root groove position of the repair shaft. When the preheating area is heated, the repair shaft needs to be rotated in order to facilitate timely monitoring of the deformation of the repair shaft.
[0126] The repaired shaft and the newly manufactured shaft head should be machined away from the bearing and preheating area and supported by supports; the repaired shaft should be rotated during heating in the preheating area to facilitate timely monitoring of the repaired shaft deformation; the heat treatment parameters during preheating are: temperature rise 80℃ / h, preheating at 350℃ for 8h; the repaired shaft rotates while heating, with a speed of 0.15r / min. After preheating, the furnace body needs to be removed, and the surrounding area of the weld should be covered with insulation materials for insulation.
[0127] (4) Welding
[0128] When welding, first perform positioning welding along the bottom of the groove weld. When positioning welding, four points must be evenly distributed, and the four-point positioning welding is symmetrical, with a welding length of 20mm. Then use the multi-layer and multi-pass welding method to weld the first to second base layers, filling layers and cover layers of the groove weld. When welding the filling layer and the cover layer, the welding must be symmetrical. The diameter of the welding rod used for the first to second base layers is smaller than that of the welding rod used for the filling layer and the cover layer. During the welding process, the interlayer temperature of the first to second base layers, the filling layer and the cover layer cannot exceed 350℃.
[0129] The welding parameters are as follows: the first and second base layers use 3.2mm diameter electrodes, the remaining filling layers and cover layers use 4mm diameter electrodes, and low current is required for welding. The interlayer temperature between layers cannot exceed 350℃. The welding parameters are as follows:
[0130] 3.2mm diameter welding rod: welding current is 120A, arc voltage is 23-24V, welding speed is 20cm / min.
[0131] 4.0mm diameter welding rod: welding current is 150A, arc voltage is 22-24V, welding speed is 29cm / min.
[0132] The deformation of the shaft end of the repaired shaft was monitored starting from the welding of the second base layer, and the deformation runout of the shaft end of the repaired shaft did not exceed 0.02mm.
[0133] (8) After welding, the repaired shaft needs to be stress-relieved by rotating and heating;
[0134] (9) The repaired shaft is rotated and placed in a local rotating preheating stress relief furnace to relieve the stress of the repaired shaft. The stress relief processing parameters of the repaired shaft are: the temperature rise of the local rotating preheating stress relief furnace is 50°C / h. When the furnace temperature of the local rotating preheating stress relief furnace is 420°C, the repaired shaft is stress relieved at 420°C, and the stress relief insulation time is 6 hours. , The repaired shaft is kept warm and then furnace cooled. When the temperature of the local rotary preheating and stress relief furnace is lower than 250°C, the repaired shaft is removed from the local rotary preheating and stress relief furnace.
[0135] (6) NDT: Clean the welding parts, polish them, and perform penetrant testing according to the drawing requirements.
[0136] (7) Post-weld processing:
[0137] After the repair shaft is welded, it is necessary to align the reserved reference surface and the journal of the repair shaft, and process the new shaft head journal. The runout value of the repair shaft is ≤0.015mm. After the journals on both sides are processed, the journals on both sides are converted to the processing reference, and then the new shaft head and welded joint are finished. Reserve 1mm margin for non-destructive testing of the new shaft head, and after passing the test, it will be finished to meet the drawing requirements.
[0138] Example 4
[0139] The only difference between Example 4 and Example 1 is that no preheating treatment is performed before welding.
[0140] Example 5
[0141] The only difference between Example 5 and Example 1 is that during welding, four-point positioning symmetrical welding is not performed, and only the multi-layer and multi-pass welding method is used to weld the first and second base layers, the filling layer and the cover layer of the groove weld.
[0142] Example 6
[0143] The only difference between Example 6 and Example 1 is that after welding, the repaired shaft needs to be subjected to stress relief under rotational heating, and the stress relief temperature is 600°C.
[0144] Performance Analysis
[0145] (1) The performance of the spindles prepared in Examples 1 to 3 was analyzed, and the analysis results are as follows:
[0146] Welding strength of the new shaft head weld: The test shows that the welding strength of the new shaft head weld is 90% of the original spindle base material strength, meeting the design requirements.
[0147] Weld quality: The weld has been tested by non-destructive testing and has no pores or slag inclusion defects, and the quality meets the requirements.
[0148] Welding deformation: After repair, the maximum runout of the shaft end is 0.013mm, which meets the design requirements.
[0149] Noise and vibration: The noise and vibration indicators of the repaired unit during operation meet the requirements.
[0150] (2) Performance Analysis of the New Spindle Prepared in Example 4 and the New Spindle Prepared in Example 1
[0151] After positioning welding, the new spindle prepared in Example 4 was found to have crack defects visible to the naked eye. The crack was located at the fusion line between the weld and the base material, and the crack extended to the base material, thus affecting the welding strength of the new spindle.
[0152] (3) Performance Analysis of the New Spindle Prepared in Example 5 and the New Spindle Prepared in Example 1
[0153] When four-point positioning is not used during welding in Example 5, the first to second base layers are directly carried out after preheating. After welding the second base layer, the shaft deformation is detected. It is found that the shaft runout of the repaired shaft exceeds the tolerance by 0.05, and the shrinkage on the side of the initial welding position is large. Therefore, it is necessary to adjust the welding sequence in reverse and perform furnace heat correction during the welding process to repair it, which increases the repair cost and repair cycle.
[0154] (4) Performance Analysis of the New Spindle Prepared in Example 6 and the New Spindle Prepared in Example 1
[0155] The new spindles obtained in Example 1 and Example 6 had no crack defects during welding and visual inspection after welding. However, in order to better remove stress, after stress relief treatment was carried out at 600°C for 4 hours in Example 6, cracks occurred in the middle part of the weld of the new spindle prepared in Example 6, resulting in failure of the repair process.
[0156] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A spindle welding repair process, characterized in that: The new spindle head and the repaired spindle are assembled into one piece by a welding repair process to form a new spindle. The welding repair process includes the following steps: A new shaft head is installed on the bearing of the repaired shaft by interference fit, and a groove weld is provided on the new shaft head; The new shaft head and the repaired shaft after hot-loading need to be preheated before welding. The preheating area is the connection area between the new shaft head and the repaired shaft including the groove weld, and avoids the blade root groove position of the repaired shaft. When the preheating area is heated, the repaired shaft needs to be rotated in order to facilitate timely monitoring of the deformation of the repaired shaft; After preheating, the repaired shaft and shaft head need to be welded. When welding, first perform positioning welding along the bottom of the groove weld. When positioning welding, four points need to be evenly distributed, and the four-point positioning welding is symmetrical; then use the multi-layer and multi-pass welding method to weld the first to second base layers, filling layers and cover layers of the groove weld. When welding the filling layer and the cover layer, the welding needs to be symmetrical. The diameter of the welding rod used for the first to second base layers is smaller than that of the welding rod used for the filling layer and the cover layer. During the welding process, the interlayer temperature of the first to second base layers, the filling layer and the cover layer cannot exceed 350℃; Monitor the deformation of the shaft end of the repaired shaft from the welding of the second base layer. When the deformation of the shaft end of the repaired shaft exceeds 0.02mm, welding is required at the reverse position of the deformation of the repaired shaft. After welding, the repaired shaft needs to be stress relieved by rotating and heating.
2. A spindle welding repair process according to claim 1, characterized in that: When the preheating area is heated, the preheating temperature is: 250°C ~ 350°C, the preheating time is 5h ~ 8h, the preheating temperature rise rate is ≤100°C / h, and the repair shaft rotation speed is 0.05r / min ~ 0.3r / min.
3. A spindle welding repair process according to claim 1, characterized in that: The first and second base layers are welded using electrodes with a diameter of 3.2 mm, and the filling layer and the cover layer are welded using electrodes with a diameter of 4.0 mm. The welding conditions are as follows: The welding current of the 3.2mm diameter electrode is 70A~120A, the arc voltage is 22V~26V, and the welding speed is 17cm / min~25cm / min; The welding current of the 4.0mm diameter electrode is 90A~150A, the arc voltage is 22V~26V, and the welding speed is 19cm / min~30cm / min.
4. A spindle welding repair process according to claim 1, characterized in that: The repaired shaft is rotated and placed in a local rotating preheating stress relief furnace to relieve the stress of the repaired shaft. The stress relief processing parameters of the repaired shaft are: the temperature rise of the local rotating preheating stress relief furnace is ≤50℃ / h. When the furnace temperature of the local rotating preheating stress relief furnace is 420℃, the repaired shaft is relieved of stress at 420℃, and the stress relief insulation time is 4h~6h , The repaired shaft is kept warm and then furnace cooled. When the temperature of the local rotary preheating and stress relief furnace is lower than 250°C, the repaired shaft is removed from the local rotary preheating and stress relief furnace.
5. A spindle welding repair process according to claim 1, characterized in that: During hot installation, the new shaft head is heated evenly, and after preheating, the groove weld connecting the new shaft head and the repaired shaft area is covered with insulation material for insulation.
6. A spindle welding repair process according to claim 1, characterized in that: Before preheating the welding part of the newly made shaft head, pre-welding preparation is required, including the following steps: (1) The welding rod pretreatment needs to be baked at 300℃~400℃ for 1h~2h and then stored at a constant temperature; (2) Determine the polarity of the welding power supply. The connection method between the welding power supply and the first to second base layers, filling layers, and cover layers should all adopt the DC reverse connection method; (3) Before welding, clean the impurities in the groove weld of the newly made shaft head so that the surface of the groove weld reveals the metallic luster.
7. A spindle welding repair process according to claim 1, characterized in that: A reference surface is set on the repair shaft near the groove weld. The reference surface of the repair shaft needs to be bright-processed before welding. The diameter of the reference surface of the repair shaft and the diameter at the weld must be close.
8. A spindle welding repair process according to claim 1, characterized in that: After welding, it is also necessary to clean the welding area, grind the welding area, and perform penetrant testing.
9. A spindle welding repair process according to claim 7, characterized in that: After the repair shaft is welded, it is necessary to align it according to the reserved reference surface and the journal of the repair shaft, and process the new shaft head and journal. The journal runout value is ≤0.02mm. After the journals on both sides are processed, convert them into processing references, and then complete the finishing of the new shaft head and welded joint.
10. A spindle welding repair process according to claim 8, characterized in that: Reserve 0.5mm to 1mm margin for non-destructive testing of welding joints.
Citation Information
Patent Citations
Cold welding and repairing technology of crankshaft cracks of large reciprocating compressor by manual argon arc welding
CN101898292A
Hollow spindle and solid spindle nose welding method
CN104785911A
Motor broken shaft reconnection technology
CN106385141A
Shaft regeneration process
CN111185714A
Electric machine axle coupling without welding broken axle
CN200990546Y
Cited By
Method for controlling butt welding straightness of thick-wall stainless steel pipes
CN119407389A
Repair and correction methods for complex machined surfaces of shaft-type workpieces
TWI912084B