Laser-assisted ultra-precision grinding process for tungsten carbide element

Through laser-assisted ultra-precision grinding process, combined with grinding wheel shaping and sharpening treatment, the accuracy and cost problems of complex curved surface processing of tungsten carbide molds are solved, and subsurface damage is repaired through laser repair technology, achieving efficient optical component production.

CN119036206AActive Publication Date: 2024-11-29GENERAL TECH GRP MASCH TOOL ENG RES INST CO LTD

Patent Information

Application Number
CN202411083512.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-29
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The prior art is difficult to achieve high-precision and low-cost complex surface processing when processing tungsten carbide molds, and efficient dressing of grinding tools and subsurface damage repair are difficult to achieve, resulting in challenges in mass production of optical components.

Method used

Using laser-assisted ultra-precision grinding process of tungsten carbide components, the precise centering of the arc center and the rotary table of the grinding wheel end is achieved by selecting suitable four-axis ultra-precision machine tools and grinding methods, combining grinding wheel shaping and sharpening treatment, and Use laser repair equipment to repair subsurface damage.

Benefits of technology

It improves processing accuracy and cost-effectiveness, reduces wear of grinding tools, significantly improves the surface quality and mechanical properties of the finished product, and extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119036206A_ABST
    Figure CN119036206A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of machining, and provides a laser-assisted ultra-precision grinding process for a tungsten carbide element, which comprises the following steps: selecting a correspondingly matched four-axis ultra-precision machine tool and a grinding mode based on the machining characteristics of a workpiece, selecting a grinding wheel type based on the grinding mode and different grinding stages, and selecting a grinding wheel type based on the grinding wheel type; each initial grinding wheel is subjected to shaping treatment and dressing treatment through a grinding rod; the workpiece is clamped on a four-axis ultra-precision machine tool, and grinding machining is conducted on the workpiece based on a preset grinding method and different working grinding wheels; and laser repairing equipment is selected based on the material characteristics of the formed element, and the laser repairing equipment is used for repairing the sub-surface damage. The initial grinding wheel is subjected to shaping treatment and dressing treatment, so that the working grinding wheel can be accurately centered, the complexity of the device is reduced, interference is avoided, errors of in-situ measurement are eliminated, subsurface damage repair on a grinding workpiece is achieved through laser repair, and the grinding precision of the workpiece is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mechanical processing, and in particular to a laser-assisted ultra-precision grinding process for a tungsten carbide component. Background Art

[0002] In recent years, small-aperture aspheric optical lenses have been increasingly widely used in the fields of smartphone lenses, vehicle-mounted imaging systems, infrared optical imaging systems, etc., due to their advantages of simplifying the structure and quality of optical systems, improving imaging quality and system resolution, and excellent optical refraction effects. Precision glass molding technology is the main technology for mass production of small-aperture aspheric optical lenses. Because precision glass molding technology is formed by replicating the surface contour of the mold, the surface accuracy and surface roughness of the mold largely determine the accuracy of the aspheric lens.

[0003] The materials of optical molding molds are usually non-metallic materials such as tungsten carbide, silicon carbide and silicon nitride, especially binder-free tungsten carbide, which not only has high hardness and high strength, but also has better wear resistance and fracture toughness than traditional tungsten carbide. It can also avoid the degradation of surface quality caused by the different thermal diffusion coefficients of binder and cemented carbide particles, and has become an ideal mold material for precision glass molding.

[0004] These molded materials usually have extremely high hardness and brittleness. The current ultra-precision cutting technologies based on single-point diamond lathes include slow-tool servo ultra-precision turning, fast-tool servo ultra-precision turning, and flying-tool turning. Due to severe tool wear during the machining process, it is impossible to achieve the machining of aspheric surfaces and other complex surfaces. Ultra-precision grinding is considered to be the main technology for machining complex surfaces on hard and brittle materials. However, requirements such as more complex surface shapes, higher machining accuracy, and more demanding surface quality have posed new challenges to the ultra-precision grinding technology of complex optical surfaces. High-precision and efficient dressing of grinding tools, full plastic domain grinding during machining, suppression or elimination of sub-surface damage of grinding workpieces, and reduction of grinding tool wear are difficult problems that researchers in this field need to solve urgently. Overcoming these problems has very important theoretical significance and application value for the mass production of complex curved optical components and promoting the development of related optical fields. Summary of the invention

[0005] The invention provides a laser-assisted ultra-precision grinding process for a tungsten carbide element, which is used to solve the defects of low machining accuracy and high machining cost in the prior art.

[0006] The invention provides a laser-assisted ultra-precision grinding process for a tungsten carbide element, comprising the following steps: selecting a corresponding matching four-axis ultra-precision machine tool and a grinding method based on the processing characteristics of a workpiece; selecting a grinding wheel based on the grinding method and different grinding stages to obtain initial grinding wheels corresponding to different grinding stages, and installing the initial grinding wheels on the four-axis ultra-precision machine tool; performing shaping and sharpening processing on each of the initial grinding wheels through a grinding rod, so that the arc center of the grinding area of ​​the processed working grinding wheel is accurately aligned with the turntable of the four-axis ultra-precision machine tool; clamping the workpiece on the four-axis ultra-precision machine tool, and grinding the workpiece based on a predetermined grinding method and different working grinding wheels, measuring the surface accuracy of the workpiece after grinding, and performing error compensation processing through the working grinding wheel until the accuracy requirement is met to obtain a molded element; selecting a laser repair device based on the material properties of the molded element itself, and using the laser emitted by the laser repair device to act on the surface of the molded element, so as to achieve repair of sub-surface damage of the molded element.

[0007] According to the laser-assisted ultra-precision grinding process of tungsten carbide components provided by the present invention, a corresponding matching four-axis ultra-precision machine tool and a grinding method are selected based on the processing characteristics of the workpiece, specifically including: selecting binderless tungsten carbide as the mold material, and based on the aspheric processing characteristics of binderless tungsten carbide, selecting the oblique axis single-point grinding method to perform grinding on the four-axis ultra-precision machine tool.

[0008] According to the laser-assisted ultra-precision grinding process of tungsten carbide elements provided by the present invention, grinding wheels are selected based on the grinding method and different grinding stages to obtain initial grinding wheels corresponding to different grinding stages, including the following steps: based on the oblique axis single-point grinding method, a metal-based diamond grinding wheel with a grain size of 400#-500# is selected as a rough grinding wheel in the rough grinding stage; a resin-based diamond grinding wheel with a grain size of 800#-1000# is selected as a semi-finishing grinding wheel in the semi-finishing grinding stage; and a ceramic-based diamond grinding wheel with a grain size of 10000#-15000# is selected as a finishing grinding wheel in the finishing grinding stage.

[0009] According to the laser-assisted ultra-precision grinding process of tungsten carbide elements provided by the present invention, the initial grinding wheel is installed on the four-axis ultra-precision machine tool, which specifically includes the following steps: the grinding spindle is installed on the turntable through the spindle sleeve and the displacement adjustment table, the displacement adjustment table can realize the precise adjustment of the grinding spindle in the three directions of X, Y and Z, and the initial grinding wheel is clamped on the grinding spindle.

[0010] According to the laser-assisted ultra-precision grinding process of tungsten carbide elements provided by the present invention, the workpiece is clamped on the four-axis ultra-precision machine tool, including the following steps: the workpiece is mounted on the workpiece spindle of the four-axis ultra-precision machine tool through a transition piece, and the circular runout of the workpiece is detected and adjusted. After passing the test, the workpiece spindle is kept in a low-speed rotation state, the workpiece is bonded and fixed, and the circular runout of the workpiece is re-checked and adjusted.

[0011] According to the laser-assisted ultra-precision grinding process of tungsten carbide elements provided by the present invention, the workpiece is ground based on a predetermined grinding method and different working grinding wheels, the surface accuracy of the workpiece after grinding is measured, and error compensation is performed by the working grinding wheel until the accuracy requirement is met to obtain a molded element, including the following steps: grinding is performed in a step-by-step grinding manner, and during specific grinding, rough grinding is performed by a metal-based diamond grinding wheel to quickly remove material excess and obtain a pre-formed curved surface; then the curved surface is semi-finished by a resin-based diamond grinding wheel, and finally fine grinding is performed by a ceramic-based diamond grinding wheel to obtain a molded element; wherein, in the fine grinding stage, after one fine grinding is completed, the surface accuracy of the fine grinding surface is measured in situ by the measuring unit integrated in the four-axis ultra-precision machine tool itself, so as to obtain a contour error, and the processing path is compensated based on the contour error until the surface accuracy of the processed surface reaches a predetermined accuracy.

[0012] According to the laser-assisted ultra-precision grinding process of tungsten carbide elements provided by the present invention, each of the initial grinding wheels is shaped and sharpened by a grinding rod, comprising the following steps: the grinding rod is mounted on the end of the workpiece spindle of the four-axis ultra-precision machine tool, and the initial grinding wheel to be processed is mounted on the turntable of the four-axis ultra-precision machine tool; the grinding spindle, the workpiece spindle and the turntable on the four-axis ultra-precision machine tool are driven to perform bevel axis grinding wheel dressing and X and Z axis interpolation dressing, so that the arc center of the grinding area of ​​the working grinding wheel is accurately aligned with the turntable.

[0013] According to the laser-assisted ultra-precision grinding process of tungsten carbide elements provided by the present invention, the grinding spindle, the workpiece spindle and the turntable on the four-axis ultra-precision machine tool are driven to perform bevel axis grinding wheel dressing and X-axis and Z-axis interpolation dressing, which specifically includes the following steps: when performing bevel axis grinding wheel dressing, the initial installation position of the initial grinding wheel shaft is located on the turntable, and the center of the small arc at the end of the initial grinding wheel is basically aligned with the center of the turntable through rough centering; then the rotary motion of the turntable is used to realize the online dressing of the grinding wheel. During the dressing process, the grinding rod rotates at a certain speed ω1, the initial grinding wheel rotates at a speed ω2, and The workpiece is fed axially along the spindle of the workpiece at a predetermined feed speed f, and the turntable drives the initial grinding wheel to rotate at the same time, so as to envelop a rounded cylindrical grinding wheel, and an arc-shaped grinding area is formed at the end of the rounded cylindrical grinding wheel; during interpolation dressing of the X and Z axes, the arc of the end of the rounded cylindrical grinding wheel is full-area color marking before dressing, and the arc of the end of the rounded cylindrical grinding wheel being dressed is always tangent to the outer arc surface of the grinding rod during the dressing process, and the rounded cylindrical grinding wheel and the grinding rod perform interpolation motion along the arc on the one hand, and on the other hand, each rotates at a certain speed so that the small arc at the end of the rounded cylindrical grinding wheel can be completely dressed.

[0014] According to the laser-assisted ultra-precision grinding process of tungsten carbide elements provided by the present invention, laser repair equipment is selected based on the material properties of the molded element itself, and the laser emitted by the laser repair equipment is used to act on the surface of the molded element to achieve sub-surface damage repair of the molded element, including the following steps: a laser drilling test is performed and the laser processing damage threshold of the molded element is obtained by extrapolation; based on the laser processing damage threshold, a suitable laser output power, scanning speed and scanning spacing are selected to perform grating scanning on the tungsten carbide surface; after the laser processing is completed, the molded element is placed in a constant temperature chamber at 20±0.5°C to cool for 25min-30min, and then placed in a sealing device filled with acetone solution, cleaned with an ultrasonic cleaner for 25min-30min to remove residual impurities on the surface, and finally placed in a sealing device filled with anhydrous ethanol, cleaned with an ultrasonic cleaner for 25min-30min, and dried to obtain a repaired molded element.

[0015] According to the laser-assisted ultra-precision grinding process of tungsten carbide elements provided by the present invention, after the repaired molding element is obtained, the repair effect of the molding element is evaluated by an evaluation method, and the evaluation method comprises the following steps: cutting is performed perpendicularly to the machining surface of the molding element before and after the repair, and two cut workpieces are obtained respectively; the cut end faces of the two cut workpieces of the molding element before the repair are placed side by side downward in a cold embedding mold for cold embedding, and the cut end faces of the two cut workpieces of the molding element after the repair are placed side by side downward in a cold embedding mold for cold embedding, one of the two cut workpieces before the repair is used as a throwaway piece, and one of the two cut workpieces after the repair is used as a throwaway piece, so as to obtain The invention discloses a method for obtaining a cold-mounted component before and after laser repair; placing the two cold-mounted components on a polishing machine to polish them to a mirror effect, and removing large-scale damage such as edge chipping and residual protrusions at the junction, as well as micro-mechanical damage; preparing a corrosion solution for the cut workpiece, and subjecting the cut workpiece to corrosion treatment for a certain period of time, so that the real sub-surface damage is fully exposed; using a transmission electron microscope to detect the sub-surface damage, and evaluating the laser repair effect according to the detection results; using a needle-tip enhanced laser confocal Raman spectroscopy system to analyze the polished surface, the ground surface and the laser repaired surface of the tungsten carbide in turn; using nano-indentation technology, evaluating the mechanical properties of the laser repaired surface, so as to realize the evaluation of the repair effect of the formed component.

[0016] The laser-assisted ultra-precision grinding process of a tungsten carbide element provided by the present invention performs shaping and sharpening treatment on the initial grinding wheel through a grinding rod, realizes the self-centering of the arc center of the end of the working grinding wheel and the turntable, eliminates the manual tool setting error, and can obtain the ideal arc radius of the end of the grinding wheel. It can be directly used in the subsequent CNC programming of ultra-precision grinding of complex curved surfaces, and no longer needs to perform in-situ measurement of the small arc at the end of the grinding wheel, which not only reduces the complexity of the device and avoids interference, but also eliminates the error of in-situ measurement, that is, the tool data is completely obtained by the machine tool system control, and the accuracy is also completely dependent on the accuracy of the machine tool. In addition, laser repair equipment is used to repair the processed molding components, which realizes the repair of sub-surface damage of the molding components, especially cracks, and improves the surface roughness, surface shape accuracy and mechanical properties, which has a great role in promoting the performance and life of the finished workpiece. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 This is one of the flow diagrams of the laser-assisted ultra-precision grinding process provided by the present invention.

[0019] Figure 2 This is the second schematic diagram of the process flow of the laser-assisted ultra-precision grinding process provided by the present invention.

[0020] Figure 3 It is a schematic flow chart of the evaluation method in the laser-assisted ultra-precision grinding process provided by the present invention.

[0021] Figure 4 It is a schematic diagram of the overall structure of a four-axis ultra-precision machine tool in the laser-assisted ultra-precision grinding process provided by the present invention.

[0022] Figure 5 It is a structural schematic diagram of a grinding rod in the laser-assisted ultra-precision grinding process provided by the present invention.

[0023] Reference numerals: 1. Workpiece spindle; 2. Grinding spindle; 3. Displacement adjustment table; 4. Turntable; 5. Machine tool body; 6. Rounded cylindrical grinding wheel; 61. Arc-shaped grinding area. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] In the description of the embodiments of the present invention, it should be noted that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present invention and simplifying the description, and do not indicate or imply that the devices or elements referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as limitations on the embodiments of the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0026] In the description of the embodiments of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "connected" and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the embodiments of the present invention can be understood according to specific circumstances.

[0027] In the embodiments of the present invention, unless otherwise clearly specified and limited, the first feature being "above" or "below" the second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, the first feature being "above", "above" and "above" the second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. The first feature being "below", "below" and "below" the second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0028] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the embodiment of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0029] In the related technology, there are many methods for repairing subsurface damage of tungsten carbide, including magnetorheological polishing, ion beam processing, HF corrosion, etc. However, these conventional subsurface damage suppression or repair methods will more or less introduce various forms of new damage and cannot achieve the ideal suppression or repair effect of subsurface damage. Therefore, laser irradiation is considered to be a more effective repair method due to its unique advantages such as high efficiency, non-contact and no introduction of new damage under suitable laser process parameters.

[0030] At present, the main methods to reduce the depth of subsurface damage include chemical mechanical polishing (CMP), magnetorheological polishing, ion beam polishing, HF etching, etc. Among them, the inevitable high normal load of chemical mechanical polishing leads to the introduction of new mechanical damage such as microcracks, fractures, and holes. Optimizing the processing technology cannot fundamentally eliminate these subsurface mechanical damages. In addition, since the material removal depth is uncontrollable, it will also lead to the deterioration of shape accuracy. The environmental pollution caused by the polishing liquid and the increase in production costs caused by the generally long polishing time are also inevitable problems.

[0031] In essence, magnetorheological polishing technology is the same as traditional polishing due to the presence of polishing liquid and polishing particles. There will also be a certain degree of hydrolysis and embedding of polishing particles on the surface. In addition, its unique magnetically sensitive particles will also be embedded in the surface of the material, which will improve the transmittance and reflective properties of the magnetorheologically polished surface while reducing the laser damage threshold. Therefore, there are certain limitations.

[0032] Ion beam processing is a method of removing sub-surface damage by combining magnetorheological polishing technology. The injection effect of bombarding ions that cannot be avoided during ion beam processing will introduce new impurities on the surface of the specimen, and the introduction of new impurities will increase the refractive index of the material surface. Therefore, it is necessary to appropriately reduce the energy of the ion beam to reduce the introduction of new impurities. However, as the impurities are reduced, the processing efficiency will also decrease. Therefore, these problems greatly limit the repair effect of sub-surface damage.

[0033] In view of the problems in the related technology, the following Figure 1 , Figure 2 The present invention describes a laser-assisted ultra-precision grinding process of a tungsten carbide component, comprising the following steps: Step S10: Select a corresponding matching four-axis ultra-precision machine tool and grinding method based on the processing characteristics of the workpiece. Specifically, the workpiece needs a corresponding matching machine tool and a corresponding grinding method under different processing characteristics. In this embodiment, the processing characteristic is ultra-precision grinding of small-diameter aspheric surfaces.

[0034] In a specific embodiment, the ultra-precision grinding process is carried out in a clean room with constant temperature and humidity, wherein Figure 4As shown, the four-axis ultra-precision machine tool includes a grinding spindle 2 and a workpiece spindle 1, the grinding spindle 2 is installed on a displacement adjustment table 3, the displacement adjustment table 3 is installed on a turntable 4, the turntable 4 is arranged on a machine tool body 5, the workpiece spindle 1 is installed on one side of the grinding spindle 2, the workpiece spindle 1 is arranged on the machine tool body 5, the workpiece spindle 1 is used to install a workpiece or a grinding rod, wherein the grinding spindle 2 is used for installing a grinding wheel, the grinding spindle 2 adopts an ultra-high-speed air-floating electric spindle with a maximum speed of 80000rpm-110000rpm, and the displacement adjustment table 3 can be fine-tuned in the X, Y, and Z directions, thereby realizing the adjustment of the grinding spindle 2 in the X, Y, and Z directions.

[0035] In this step, it is necessary to select the workpiece material, that is, the mold material. Specifically, binderless tungsten carbide is selected as the mold material, and based on the aspheric processing characteristics of binderless tungsten carbide, the oblique axis single point grinding method is selected to perform grinding on a four-axis ultra-precision machine tool.

[0036] It is understandable that among various mold materials, binderless tungsten carbide has higher hardness, wear resistance, fracture toughness and chemical stability, so it has better processing performance. At the same time, it can effectively avoid the degradation of workpiece surface quality caused by the different thermal diffusion coefficients of binders such as Co or Ni and cemented carbide particles. Therefore, M78 binderless tungsten carbide is selected as the mold material, and the workpiece size is Φ25mmX10mm.

[0037] The grinding method selected is the oblique axis single-point grinding method, which can achieve deterministic precision removal of aspheric surfaces and is suitable for ultra-precision grinding of small-diameter aspheric surfaces. Among them, the oblique axis single-point grinding is point contact, and the grinding wheel is a right-angle cylindrical grinding wheel or a rounded cylindrical grinding wheel. In this manual, the rounded cylindrical grinding wheel is used for explanation. During the processing, the axis of the grinding wheel is coplanar with the axis of the workpiece and there is a fixed angle. The single-point contact between the grinding wheel and the aspheric workpiece is achieved by controlling the rotation angle of the grinding axis, while ensuring that the grinding point of the grinding wheel is always perpendicular to the normal of the workpiece grinding point.

[0038] Step S20, select the grinding wheel based on the grinding method and different grinding stages, obtain the initial grinding wheel corresponding to the different grinding stages, and install the initial grinding wheel on the four-axis ultra-precision machine tool. Different grinding methods and different grinding stages require the selection of different initial grinding wheels. The selection of the grinding wheel can achieve the matching of the grinding method and the grinding stage, so as to achieve ultra-precision grinding of the workpiece.

[0039] According to the grinding method used (oblique axis single point grinding method, and grinding by step-by-step grinding method) and the tool clamping method of the grinding spindle 2, a rounded cylindrical grinding wheel 6 is designed. The parameters of the initial grinding wheel are selected as follows: Abrasive selection: Abrasive is the main raw material of grinding wheel. Since ordinary abrasives such as corundum and silicon nitride are not suitable for ultra-precision grinding of hard and brittle materials, diamond abrasive grinding wheel is selected.

[0040] Binder selection: Binder is one of the components of the grinding wheel, used to consolidate the abrasive, and plays a decisive role in the strength, impact resistance, heat resistance and other properties of the grinding wheel. Metal bond grinding wheels are selected for rough grinding due to their good wear resistance; resin bond grinding wheels and vitrified bond grinding wheels are mainly used to ensure surface roughness during the grinding process, so resin bond grinding wheels and vitrified bond grinding wheels are selected for semi-finishing and fine grinding processes.

[0041] Grain size selection: Grain size refers to the size of abrasive particles. A metal-based diamond grinding wheel with a grain size of 400#-500# is used as a rough grinding wheel. The grinding allowance is large during rough grinding. Coarser abrasive grains are used. The abrasive grains are coarse and the pores are large. The grinding depth can be larger, the processing allowance can be removed faster, and the grinding wheel is not easy to clog and heat up, thereby improving the efficiency of the grinding process; for semi-finishing grinding, a resin-based diamond grinding wheel with a grain size of 800#-1000# is used as a semi-finishing grinding wheel to achieve the transition process between rough grinding and fine grinding. It is necessary not only to remove the visual surface damage caused by large grain size and large grinding depth in rough grinding, but also to take into account the processing efficiency; for fine grinding, a ceramic-based diamond grinding wheel with a grain size of 10000#-15000# is used as a fine grinding wheel. The processing allowance is small during fine grinding and the roughness value is required to be lower. This requirement can be met by selecting finer abrasive grains.

[0042] S30, shaping and sharpening each initial grinding wheel by a grinding rod, so that the arc center of the grinding area of ​​the processed working grinding wheel is precisely aligned with the turntable 4 of the four-axis ultra-precision machine tool.

[0043] Grinding tools are an important factor affecting the final workpiece surface forming quality and the stability of the entire machining process. If necessary, the initial grinding wheel needs to be precisely dressed in situ. Grinding wheel dressing is divided into two processes: shaping and sharpening. The former is to maintain the correct geometric shape of the grinding wheel, and the latter is to make the abrasive protrude and improve the grinding efficiency. The dressing process is as follows.

[0044] Installation of grinding spindle 2: The grinding spindle 2 is installed on the turntable 4 through the spindle sleeve and the displacement adjustment table 3. The displacement adjustment table 3 can realize the precise adjustment of the grinding spindle 2 in the three directions of X, Y and Z. In the specific example, the grinding spindle 2 adopts an ultra-high-speed air-floating electric spindle.

[0045] Grinding wheel dressing process: In view of the non-spherical processing characteristics of typical processing samples, the in-situ precision dressing method of the outer cylindrical surface of the rotating green silicon carbide (GC) grinding rod is selected. The initial grinding wheel dressing is carried out before clamping the workpiece, wherein the green silicon carbide (GC) grinding rod is installed at the end of the workpiece spindle 1, and it is clamped by an ER chuck (elastic chuck with a round handle), which can be connected to the spindle by threaded connection or hot fitting; the initial grinding wheel is installed on an ultra-high-speed air-floating electric spindle. Among them, the ER chuck is a common clamping tool, and its specific clamping method and specific mechanism will not be repeated. During the dressing process, the water-based grinding fluid or oil-based grinding fluid remains in the open state, and the grinding wheel dressing is carried out in the following two steps: Bevel grinding wheel dressing: The grinding wheel axis (i.e., grinding spindle 2) is installed on turntable 4. After rough centering, the center of the small arc at the end of the initial grinding wheel is basically aligned with the center of turntable 4 (rough centering); then the rotary motion of turntable 4 is used to achieve online dressing of the grinding wheel: during the dressing process, the grinding rod rotates at a certain speed ω1, the grinding wheel rotates at a suitable speed ω2, and feeds axially along the workpiece spindle 1 at a certain feed speed f. At the same time, turntable 4 drives the initial grinding wheel to rotate, enveloping the arc-shaped grinding area 61 (the small arc area at the end) of the rounded cylindrical grinding wheel 6 (i.e., the working grinding wheel). After one cycle of axial feeding, the processed grinding wheel is fed radially, and the dressing depth of the grinding wheel gradually increases. Since the formation of the arc is driven by turntable 4, the center of the arc at the end of the dressed grinding wheel is naturally aligned with the rotation center of turntable 4, so there is no need for alignment operation, eliminating the tool setting error of this part.

[0046] X, Z axis interpolation dressing: Using the X, Z axis linkage function, the grinding rod interpolates and dresses the diamond grinding wheel to form an arc. Before dressing, the arc at the end of the rounded cylindrical grinding wheel 6 (i.e., the working grinding wheel) is marked with full-area color. During the dressing process, the arc at the end of the working grinding wheel being dressed is always tangent to the outer arc surface of the grinding rod. On the one hand, the grinding wheel and the grinding rod perform interpolation motion along the arc, and on the other hand, they rotate at a certain speed to ensure the complete dressing of the small arc at the end of the grinding wheel, so as to improve the arc dressing accuracy of the grinding wheel.

[0047] In a specific example, one interpolation movement of the diamond grinding wheel during the interpolation dressing process is a dressing cycle. After one dressing cycle is completed, the diamond grinding wheel is fed to a certain depth ap along the interpolation radius direction, and the arc profile of the dressing grinding wheel is obtained through the mutual wear between the green silicon carbide rod and the diamond grinding wheel until the color mark at the arc at the end of the grinding wheel completely disappears, and the interpolation dressing is completed. Among them, the relationship between the radii involved in the diamond wheel dressing process during the interpolation dressing process is: R=r0+r (where R is the interpolation arc radius, r0 is the radius of the green silicon carbide rod used for dressing, and r is the arc radius of the end of the working grinding wheel after dressing). The interpolation arc radius needs to be corrected after each interpolation dressing cycle. The corrected interpolation arc radius is R-ap. The r obtained in this way is the arc radius of the end of the working grinding wheel after dressing, which can be directly used in the subsequent CNC programming of ultra-precision grinding of complex surfaces. There is no need to perform in-situ measurement of the small arc at the end of the grinding wheel, which reduces the complexity of the device, avoids interference, and eliminates the error of in-situ measurement. That is, the tool data is completely obtained by the machine tool system, and the accuracy depends entirely on the machine tool accuracy.

[0048] By combining the above two grinding wheel dressing methods, the arc center of the working grinding wheel grinding area can be accurately aligned with the turntable 4, eliminating the angle compensation of the turntable 4 during the grinding process, and can also achieve accurate dressing of the working grinding wheel to obtain the precise arc radius of the working grinding wheel end, providing a basis for subsequent ultra-precision grinding of complex surfaces.

[0049] Step S40: clamp the workpiece on a four-axis ultra-precision machine tool, and grind the workpiece based on a predetermined grinding method and different working grinding wheels, measure the surface accuracy of the workpiece after grinding, and perform error compensation processing through the working grinding wheel until the accuracy requirement is met to obtain a molded component. Different working grinding wheels need to be replaced for grinding at different grinding stages, as follows: Workpiece clamping: Due to the small size of the workpiece, a clamping assembly (not shown in the figure) is designed. The clamping assembly includes a transition piece, a transition plate and a vacuum suction cup. The transition piece is used to clamp the workpiece. The transition plate is installed at the front end of the vacuum suction cup, and a small hole is opened in the center of the transition plate for ventilation. When the workpiece is clamped, the transition piece is installed on the transition plate at the front end of the vacuum suction cup with screws and its circular runout is adjusted. At this time, the vacuum pump is in the on state, and the vacuum pump is connected to the small hole to adsorb the workpiece on the transition piece, and the circular runout of the workpiece is detected and adjusted. After passing the test, the workpiece spindle 1 is kept in a low-speed rotation state, the workpiece is bonded and fixed, and the circular runout of the workpiece is re-checked and adjusted. After the bonding is firm, the vacuum pump is disconnected. During the grinding process, the vacuum pump is in the off state to suppress the vibration caused by the gas source and ensure the surface processing quality.

[0050] Grinding: Grinding adopts a step-by-step grinding method. The specific process is divided into three stages: rough grinding, semi-finishing grinding, and fine grinding. The grinding conditions and process parameters of the three stages are shown in the following table. Since the grinding wheels with different grits and binders need to be replaced in the three stages, the rough centering and dressing of the grinding wheels need to be performed separately. First, a metal-based diamond grinding wheel with a grit of 400# is used for rough grinding to quickly remove the excess material and obtain a preformed curved surface; in the semi-finishing and fine grinding stages, a small-grained grinding wheel is used to ensure the required surface accuracy and surface quality. Among them, in the fine grinding stage, after one fine grinding is completed, the measuring unit (ie, LVDT) integrated in the machine tool itself is used to measure the surface accuracy of the fine grinding surface in situ, so as to obtain the contour error, and the processing path of the grinding wheel is compensated based on this, and the ultra-precision grinding-surface accuracy measurement-error compensation cycle is carried out until the surface accuracy of the machined surface meets the requirements. After the fine grinding is completed, the surface roughness of the fine grinding is obtained by laser interferometer detection.

[0051] The specific grinding process parameters are as follows:

[0052] Step S50: Select laser repair equipment based on the material properties of the molding element itself, and use the laser emitted by the laser repair equipment to act on the surface of the molding element to repair the sub-surface damage of the molding element. The molding element itself causes a lot of sub-surface damage during the grinding process. The present invention uses laser repair equipment to repair it, as follows: Rough grinding of tungsten carbide causes many surface layer damages, such as microcracks, lattice distortion, etc., with a depth of about 20~30μm. The removal of these surface layer damages is achieved by subsequent fine grinding. At the same time, fine grinding will also lead to a thinner subsurface damage layer, mainly including microcracks, amorphous layers, dislocations, stacking faults, etc. The existence of these damages will not only lead to a decrease in surface mechanical properties, but also when the depth of the damage layer exceeds the surface shape accuracy, the surface shape accuracy loses its reference value; and too deep subsurface damage will also greatly increase post-processing work and reduce processing efficiency. Therefore, it is very important to reduce or suppress subsurface damage.

[0053] Based on this, a method of using laser to repair subsurface damage of tungsten carbide is proposed, which can achieve efficient and high-quality repair of subsurface damage without material removal and environmental pollution. According to the different pulse widths, commonly used lasers mainly include millisecond, nanosecond, subnanosecond, femtosecond, picosecond, etc. Nanosecond lasers have many advantages over other lasers, such as wide material application range, high material removal rate, and moderate equipment cost. Nanosecond lasers are used here for damage repair, and a laser repair evaluation method for subsurface damage is established to evaluate the repair effect.

[0054] When the laser acts on the tungsten carbide surface, the instantaneous high energy absorption will increase the local temperature of the laser action area on its surface. With the cumulative effect of the pulse, the surface temperature continues to rise until it reaches the melting point of tungsten carbide. At this time, the material in the laser action area changes from solid to molten. If the pulse laser continues to act, the temperature will continue to rise due to the accumulation of energy until it reaches its surface vaporization temperature. The temperature variation range during the laser repair process is exactly the temperature range between the melting temperature and the vaporization temperature. Within this temperature range, tungsten carbide melts to a certain depth, so that its surface and subsurface micro-damage within this depth range melts together. With the end of the laser pulse action, the material gradually cools down. Damage such as microcracks is repaired during the cooling and recrystallization process, and the lattice structure will also change accordingly. At the same time, the tip stress of the crack is also reduced. This patent selects the grating line scanning method for subsurface damage repair.

[0055] Laser repair equipment: The laser repair system mainly consists of precision displacement platform (three-axis displacement platform), nanosecond laser, reflector, shutter, Glan prism, beam expander and other optical components. Other optical components can be added as needed.

[0056] The laser repair process route and evaluation method are as follows: Determine the damage threshold of tungsten carbide laser processing: The laser beam propagation used satisfies the Gaussian beam propagation characteristics, that is, the laser energy satisfies the Gaussian distribution function in the spatial position, and the beam cross-sectional radius in the laser propagation direction and the beam propagation displacement also satisfy the Gaussian function.

[0057] Specifically, based on the laser repair mechanism of tungsten carbide, obtaining the laser processing damage threshold is the basis of repair. The damage threshold is obtained by extrapolation through laser drilling test. The tungsten carbide workpiece is placed at the focal plane with zero defocus, and a water jet device is set to assist in processing. The relative position of the nozzle and the laser focal plane is fixed during the processing to avoid introducing new influencing factors and causing deviations in the final results. Tungsten carbide is punched at different powers and action times to ensure that stable small hole ablation can be achieved within a short dwell time under the selected power. The ablation aperture size at different powers and different dwell times is measured using a scanning electron microscope (SEM). Since the ablation aperture size of the laser on the material is linearly related to the logarithm of the laser power, a functional relationship between the laser output power and the aperture is established, and then the corresponding laser processing damage threshold is calculated by an empirical formula.

[0058] Laser repair of tungsten carbide: Select appropriate laser output power, scanning speed and scanning spacing to perform raster-line scanning on the surface of tungsten carbide. The principle of selecting the scanning spacing is to keep it as small as possible while ensuring sufficient processing efficiency. After the laser processing is completed, the tungsten carbide workpiece is placed in a constant temperature chamber at 20±0.5℃ to cool for 25min-30min, and then placed in a sealed device filled with acetone solution and cleaned with an ultrasonic cleaner for 25min-30min to remove residual impurities on the surface. Finally, it is placed in a sealed device filled with anhydrous ethanol and cleaned with an ultrasonic cleaner for 25min-30min. After it is dried, the surface morphology of the processed surface is observed and the surface roughness is analyzed using instruments such as a transmission electron microscope (TEM) and a white light interferometer, and then the damage repair effect is preliminarily analyzed.

[0059] like Figure 3 As shown, the evaluation is performed by the constructed evaluation method. Specifically, the evaluation of the laser repair effect of the tungsten carbide workpiece is as follows: In order to more intuitively reflect the laser repair effect of the tungsten carbide workpiece, the following evaluation method is established for the workpiece after laser repair: Cold embedding: Cut the tungsten carbide workpieces before and after repair into two pieces vertically along the repair surface (i.e., the grinding surface of the workpiece) to obtain two cut workpieces (two cut workpieces before and two cut workpieces after repair). Place the cut end faces of the two cut workpieces before repair side by side downward in a cold embedding mold for cold embedding. Place the cut end faces of the two cut workpieces after repair side by side downward in a cold embedding mold for cold embedding. Use one of the two cut workpieces before repair as a throwaway piece and one of the two cut workpieces after repair as a throwaway piece, where the throwaway piece is used to reduce the edge effect, to obtain one tungsten carbide cold embedding piece before and after laser repair.

[0060] Polishing: Place the two cold-mounted parts on a polishing machine and polish them to a mirror finish, removing large-scale damage such as edge chipping and residual protrusions at the junction, as well as minor mechanical damage.

[0061] Polishing surface corrosion: Prepare tungsten carbide corrosion solution and perform corrosion treatment for a certain period of time to fully expose the real sub-surface damage, especially cracks. The corrosion time is determined by the microscopic observation images of the morphology of the same crack after corrosion from short to long time. After the corrosion is completed, the sample should be cleaned immediately with acetone and deionized water to prevent the residual corrosion solution on the surface from continuing to corrode the sample, thereby prolonging the corrosion time.

[0062] Subsurface damage detection and evaluation: 1) Use a transmission electron microscope to detect subsurface damage, and evaluate the laser repair effect based on the detection results (compare and analyze the detection results of the polished workpiece before and after the repair). The repair effect obtained in this embodiment is: under appropriate laser output power and scanning speed, the subsurface crack depth of the tungsten carbide workpiece after laser repair is reduced, and the crack tip temperature is increased to its melting temperature under the action of the pulsed laser, so that the surface and subsurface micro-damage of the tungsten carbide workpiece are melted together, and the stress concentration at the crack tip is greatly reduced, which has a good inhibitory effect on the expansion of the crack. It can be said that laser repair achieves a certain degree of micro-crack healing, and further plays a role in crack arrest.

[0063] 2) The tip-enhanced laser confocal Raman spectroscopy system was used to analyze the polished surface, ground surface and laser repaired surface of tungsten carbide in turn. The analysis results obtained in this example show that the Raman spectrum obtained from the polished surface of the cut workpiece is very similar to the spectrum of the laser repaired surface, that is, the polishing process does not introduce new amorphous layer defects.

[0064] 3) Nanoindentation technology is used to evaluate the mechanical properties of the laser repaired surface. The analysis results obtained in this example show that the surface after laser repair has a higher fracture limit, and the plastic domain processing range is widened, which is more conducive to the subsequent processing and application of tungsten carbide.

[0065] In summary, it can be seen that compared with the existing ultra-precision grinding process for hard and brittle materials, the process scheme of the present invention is more comprehensive, and higher grinding processing accuracy can be guaranteed through the effective implementation of various technical points; further, the two dressing methods are combined during grinding wheel dressing, achieving the basic purpose of grinding wheel dressing - grinding wheel shaping and sharpening, and secondly, the self-centering of the end arc center and the turntable 4 is achieved, eliminating the manual tool setting error, and finally the ideal grinding wheel end arc radius can be obtained, which can be directly used in the subsequent CNC programming of ultra-precision grinding of complex curved surfaces, without the need to perform in-situ measurement of the small arc at the end of the grinding wheel, which not only reduces the complexity of the device and avoids interference, but also eliminates the error of in-situ measurement, that is, the tool data is completely obtained by the machine tool system control, and the accuracy is also completely dependent on the machine tool accuracy. Further, for the repair process of sub-surface damage of tungsten carbide workpieces after ultra-precision grinding, the laser repair method and repair effect evaluation system established by the present invention can effectively realize the repair of sub-surface damage, especially cracks, and improve the surface roughness, surface accuracy and mechanical properties, which has a great driving effect on the performance and life of related workpieces.

[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A laser-assisted ultra-precision grinding process for tungsten carbide components, characterized in that: The following steps are involved: Select the corresponding four-axis ultra-precision machine tool and grinding method based on the processing characteristics of the workpiece; Selecting a grinding wheel based on the grinding method and different grinding stages to obtain initial grinding wheels corresponding to different grinding stages, and installing the initial grinding wheels on the four-axis ultra-precision machine tool; Performing shaping and sharpening treatment on each of the initial grinding wheels by means of a grinding rod, so that the arc center of the grinding area of ​​the processed working grinding wheel is precisely aligned with the turntable of the four-axis ultra-precision machine tool; The workpiece is clamped on the four-axis ultra-precision machine tool, and the workpiece is ground based on a predetermined grinding method and different working grinding wheels, the surface accuracy of the workpiece after grinding is measured, and error compensation is performed by the working grinding wheel until the accuracy requirement is met to obtain a molded component; A laser repair device is selected based on the material properties of the molding element itself, and the laser emitted by the laser repair device is used to act on the surface of the molding element to repair the sub-surface damage of the molding element.

2. The laser-assisted ultra-precision grinding process of tungsten carbide components according to claim 1, characterized in that: Based on the processing characteristics of the workpiece, the corresponding matching four-axis ultra-precision machine tool and grinding method are selected, including: Binderless tungsten carbide is selected as the mold material. Based on the aspheric processing characteristics of binderless tungsten carbide, the oblique axis single-point grinding method is selected to perform the grinding process on the four-axis ultra-precision machine tool.

3. The laser-assisted ultra-precision grinding process of tungsten carbide components according to claim 2, characterized in that: Grinding wheel selection is performed based on the grinding method and different grinding stages to obtain initial grinding wheels corresponding to different grinding stages, including the following steps: Based on the oblique axis single-point grinding method, a metal-based diamond grinding wheel with a grain size of 400#-500# is selected as a rough grinding wheel in the rough grinding stage; a resin-based diamond grinding wheel with a grain size of 800#-1000# is selected as a semi-finishing grinding wheel in the semi-finishing grinding stage; and a ceramic-based diamond grinding wheel with a grain size of 10000#-15000# is selected as a fine grinding wheel in the fine grinding stage.

4. The laser-assisted ultra-precision grinding process of tungsten carbide components according to claim 3, characterized in that: The initial grinding wheel is installed on the four-axis ultra-precision machine tool, specifically comprising the following steps: The grinding spindle is installed on the turntable through a spindle sleeve and a displacement adjustment table. The displacement adjustment table can realize precise adjustment of the grinding spindle in three directions of X, Y and Z. The initial grinding wheel is clamped on the grinding spindle.

5. The laser-assisted ultra-precision grinding process of tungsten carbide components according to claim 2, characterized in that: Clamping the workpiece on the four-axis ultra-precision machine tool comprises the following steps: The workpiece is mounted on the workpiece spindle of the four-axis ultra-precision machine tool through a transition piece, and the circular runout of the workpiece is detected and adjusted. After passing the test, the workpiece spindle is kept in a low-speed rotation state, the workpiece is bonded and fixed, and the circular runout of the workpiece is re-checked and adjusted.

6. The laser-assisted ultra-precision grinding process of tungsten carbide components according to claim 1, characterized in that: The workpiece is ground based on a predetermined grinding method and different working grinding wheels, the surface accuracy of the workpiece after grinding is measured, and error compensation is performed by the working grinding wheel until the accuracy requirement is met to obtain a molding element, including the following steps: The grinding process is carried out in a step-by-step grinding manner. During the specific grinding, rough grinding is performed by a metal-based diamond grinding wheel to quickly remove the excess material and obtain a pre-formed curved surface; then the curved surface is semi-finished by a resin-based diamond grinding wheel, and finally fine grinding is performed by a ceramic-based diamond grinding wheel to obtain a formed component; Among them, in the fine grinding stage, after one fine grinding is completed, the measuring unit integrated in the four-axis ultra-precision machine tool is used to measure the surface accuracy of the fine grinding surface in situ, so as to obtain the contour error, and the processing path is compensated based on the contour error until the surface accuracy of the processed surface reaches the predetermined accuracy.

7. The laser-assisted ultra-precision grinding process of tungsten carbide components according to claim 1, characterized in that: The process of shaping and sharpening each of the initial grinding wheels by means of a grinding rod comprises the following steps: The grinding rod is mounted on the end of the workpiece spindle of the four-axis ultra-precision machine tool, and the initial grinding wheel to be processed is mounted on the turntable of the four-axis ultra-precision machine tool; The grinding spindle, workpiece spindle and turntable on the four-axis ultra-precision machine tool are driven to perform bevel grinding wheel dressing and X-axis and Z-axis interpolation dressing, so that the arc center of the grinding area of ​​the working grinding wheel is accurately aligned with the turntable.

8. The laser-assisted ultra-precision grinding process of tungsten carbide components according to claim 7, characterized in that: Driving the grinding spindle, workpiece spindle and turntable on the four-axis ultra-precision machine tool to perform bevel axis grinding wheel dressing and X-axis and Z-axis interpolation dressing specifically includes the following steps: When performing the dressing of the bevel-axis grinding wheel, the initial installation position of the initial grinding wheel shaft is located on the turntable, and the center of the small arc at the end of the initial grinding wheel is basically aligned with the center of the turntable through rough centering; then the online dressing of the grinding wheel is realized by the rotary motion of the turntable. During the dressing process, the grinding rod rotates at a certain speed ω1, the initial grinding wheel rotates at a speed ω2, and is fed axially along the workpiece spindle at a predetermined feed speed f, and at the same time, the turntable drives the initial grinding wheel to rotate, enveloping a rounded cylindrical grinding wheel, and a circular arc grinding area is formed at the end of the rounded cylindrical grinding wheel; During interpolation dressing of the X and Z axes, the entire area is color-marked at the arc at the end of the rounded cylindrical grinding wheel before dressing. During the dressing process, the arc at the end of the rounded cylindrical grinding wheel being dressed is always tangent to the outer arc surface of the grinding rod. On the one hand, the rounded cylindrical grinding wheel and the grinding rod perform interpolation motion along the arc, and on the other hand, each rotates at a certain speed, so that the small arc at the end of the rounded cylindrical grinding wheel can be completely dressed.

9. The laser-assisted ultra-precision grinding process of tungsten carbide components according to claim 1, characterized in that: Selecting a laser repair device based on the material properties of the molding element itself, and using the laser emitted by the laser repair device to act on the surface of the molding element to repair the sub-surface damage of the molding element, includes the following steps: The laser processing damage threshold of the formed component is obtained by using a laser drilling test and an extrapolation method; Based on the laser processing damage threshold, a suitable laser output power, scanning speed and scanning spacing are selected to perform grating scanning on the tungsten carbide surface; After the laser processing is completed, the molded component is placed in a constant temperature chamber at 20±0.5°C to cool for 25min-30min, then placed in a sealed device filled with acetone solution, cleaned with an ultrasonic cleaner for 25min-30min to remove residual impurities on the surface, and finally placed in a sealed device filled with anhydrous ethanol, cleaned with an ultrasonic cleaner for 25min-30min, and dried to obtain the repaired molded component.

10. The laser-assisted ultra-precision grinding process of tungsten carbide components according to claim 9, characterized in that: After the repaired molding element is obtained, the repair effect of the molding element is evaluated by an evaluation method, and the evaluation method comprises the following steps: Cutting perpendicularly to the machined surface of the molding element before and after repair, and obtaining two cut workpieces respectively; The cut end faces of the two cut workpieces of the molding element before repair are placed side by side downward in a cold embedding mold for cold embedding, and the cut end faces of the two cut workpieces of the molding element after repair are placed side by side downward in a cold embedding mold for cold embedding, one of the two cut workpieces before repair is used as a throwaway piece, and one of the two cut workpieces after repair is used as a throwaway piece, so as to obtain one cold embedding piece before laser repair and one cold embedding piece after laser repair; The two cold-mounted parts are placed on a polishing machine and polished to a mirror effect, and large-scale damage such as edge chipping and residual protrusions at the junction and minor mechanical damage are removed; A corrosive solution is prepared for the cut workpiece, and the cut workpiece is corroded for a certain period of time so that the real sub-surface damage is fully exposed; A transmission electron microscope was used to detect sub-surface damage and the laser repair effect was evaluated based on the test results. The polished surface, ground surface and laser repaired surface of tungsten carbide were analyzed in turn using a needle-tip enhanced laser confocal Raman spectroscopy system. The mechanical properties of the laser repaired surface were evaluated using nanoindentation technology to evaluate the repair effect of the molded components.

Citation Information

Patent Citations

  • Single-direction inclined-shaft profiling precision grinding method of array optical elements of micro circular troughs

    CN102513899A

  • Quartz glass ductile-regime grinding method based on laser crack pre-repairing

    CN104385065A

  • Ultraprecision grinding method for resin-based diamond abrasive wheel having rotating-shaft-symmetric continuous surface

    CN106625036A

  • Ultra-precision grinding method for surface of tungsten carbide or silicon carbide workpiece

    CN115890355A

  • Grinding wheel dressing device of grinding machine

    CN118404504A

Cited By

  • Weak-rigidity free-form surface monocrystalline silicon reflecting lens and processing method thereof

    CN119635852A

  • Four-axis linkage ultraprecise turning method for hard and brittle materials

    CN121316118A

  • Polishing method for Parylene coating on surface of medical puncture needle, medical puncture needle and device

    CN122626066A