Method for continuously preparing micro-nano iron phosphate, micro-nano iron phosphate and application

By using a continuous method to prepare micro-nano ferric phosphate, the reaction raw material solution and pH adjuster are simultaneously introduced into pure water to control the precipitation process and avoid agglomeration. This solves the problems of consistency and high cost of ferric phosphate in existing processes, and realizes efficient and environmentally friendly industrial production.

CN119038508APending Publication Date: 2024-11-29湖北金泉新材料有限公司

Patent Information

Application Number
CN202411167650.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing batch processes for preparing iron phosphate are complex, produce poor product consistency, are prone to agglomeration, have low tap density, are difficult to automate, are costly, and are neither environmentally friendly nor economically viable.

Method used

A continuous method for preparing micro-nano iron phosphate was adopted. The reaction raw material solution and pH adjuster were simultaneously introduced into pure water to carry out the precipitation reaction. The low supersaturation concentration environment was controlled to avoid agglomeration, simplify the process, omit the Fe2+ pre-oxidation step, and use surfactants to disperse the particles.

Benefits of technology

It improves the tap density and product consistency of ferric phosphate, simplifies the process, reduces costs, improves production efficiency and material purity, and enables industrial application and automatic control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038508A_ABST
    Figure CN119038508A_ABST
Patent Text Reader

Abstract

The invention provides a method for continuously preparing micro-nano iron phosphate, micro-nano iron phosphate and application, and the method comprises the following steps: simultaneously introducing a reaction raw material solution and a pH regulator into pure water, carrying out a precipitation reaction, and then sequentially carrying out an aging reaction and calcination to obtain the micro-nano iron phosphate, wherein the reaction raw material solution comprises an iron source and a phosphorus source. The process method disclosed by the invention is a continuous process, so that agglomeration of formed iron phosphate can be avoided, and the tap density is improved; the process is simplified, acid and alkali are saved, the raw material utilization rate is high, the cost is reduced, the production efficiency is improved, environmental protection is achieved, meanwhile, the product consistency is good, and industrial application can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries and relates to a method for continuously preparing micro-nano iron phosphate, the micro-nano iron phosphate and applications. Background Art

[0002] At present, the process for preparing ferric phosphate is usually to use FeSO4·7H2O as the iron source, prepare an aqueous solution, add acid to acidify, then add an excess of oxidant, then add a certain amount of phosphoric acid or phosphate, adjust the pH value with alkali, so that trivalent iron ions and phosphate ions combine to form a precipitate, and obtain crystalline FePO4·2H2O through washing and aging, and then obtain anhydrous FePO4 through high-temperature roasting and dehydration. The above process is an intermittent operation process. The above process is an intermittent process, the preparation process is relatively long and complicated, the consistency of the product is not good enough, the particles are prone to agglomeration, resulting in a low tap density, and the embedding and extraction of lithium ions in LiFePO4 will be affected after it is made; and automated production is difficult to achieve, the industrial production cost is high, and a large amount of acid, alkali and oxidant will be consumed, and a large amount of wastewater will be generated, which is poor in economy and environmental protection. Therefore, it is urgent to provide a process for preparing ferric phosphate that can solve the above problems. Summary of the invention

[0003] In view of the shortcomings of the prior art, the present invention aims to provide a method for continuously preparing micro-nano iron phosphate, micro-nano iron phosphate and its application. The process of the present invention is a continuous process, which is easy to operate, environmentally friendly and economical, can avoid the agglomeration of the formed iron phosphate and improve the tap density; and, Fe is omitted. 2+ The pre-oxidation step simplifies the process while saving acid and alkali, high raw material utilization, reduced costs, improved production efficiency and environmental protection. At the same time, the finished material has high purity, excellent performance, good product consistency, can be industrialized and easy to control automatically.

[0004] To achieve this object, the present invention adopts the following technical solutions:

[0005] In a first aspect, the present invention provides a method for continuously preparing micro-nano iron phosphate, the method comprising:

[0006] The reaction raw material liquid and the pH regulator are simultaneously introduced into pure water to perform a precipitation reaction, and then an aging reaction and calcination are performed in sequence to obtain micro-nano iron phosphate;

[0007] Wherein, the reaction raw material liquid includes an iron source and a phosphorus source.

[0008] It should be noted that “the reaction raw material liquid and the pH adjuster are introduced simultaneously” means that the reaction raw material liquid and the pH adjuster are introduced at the same time and are introduced at the same time.

[0009] The present invention provides a method for continuously preparing micro-nano iron phosphate, wherein pure water is used as a base liquid, a co-precipitation environment with a low supersaturation concentration can be created, and a crystallization process can be better controlled; a reaction raw material liquid and a pH regulator are introduced simultaneously in order to cooperate with the pure water base liquid, the reaction raw material liquid and the pH regulator are introduced into the pure water at the same time, and precipitation is continuously generated in the pure water, and agglomeration of the generated precipitation can be avoided as much as possible, and the overall precipitation process is carried out in an environment with a low supersaturation concentration, which is conducive to the preparation of micro-nano iron phosphate with good crystallinity; compared with directly adding a pH regulator to the reaction raw material liquid, the method of adding the reaction raw material liquid and the pH regulator to the pure water at the same time can better control the binding rate of iron ions and phosphates in the precipitation process, avoid agglomeration of the formed iron phosphate, and thus improve the tap density of the final iron phosphate product;

[0010] The process of the present invention is a continuous process, which is easy to operate, environmentally friendly and economical. The prepared iron phosphate can reach the micro-nano level. 2+ The pre-oxidation step simplifies the process while saving acid and alkali, high raw material utilization, reduced costs, improved production efficiency and environmental protection. At the same time, the finished material has high purity, excellent performance, good product consistency, can be industrialized and easy to control automatically.

[0011] It should be explained that the amorphous iron phosphate precursor obtained by the precipitation reaction of the present invention is mainly a yellow-brown precipitate mixture of FePO4 and Fe(OH)3. Subsequently, Fe(OH)3 and phosphoric acid are reacted by aging reaction to generate iron phosphate and a crystal transformation occurs to obtain crystalline iron phosphate dihydrate, and the color also changes to white-pink. It is then calcined to remove moisture to obtain micro-nano iron phosphate.

[0012] Preferably, the pure water is contained in the reactor, and the volume of the pure water is 10 to 20% of the volume of the reactor, for example, it can be 10%, 12%, 15%, 18% or 20%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0013] Preferably, the iron source comprises iron salts and / or iron oxides.

[0014] Preferably, the iron salt comprises at least one of Fe2(SO4)3, Fe(NO3)3 and FeCl3, preferably Fe(NO3)3.

[0015] Preferably, the iron oxide comprises Fe2O3.

[0016] Optionally, the iron salt is a hydrated iron salt, including at least one of FeSO4·7H2O, Fe(NO3)3·9H2O, FeCl3·6H2O and Fe2O3, preferably Fe(NO3)3·9H2O.

[0017] Preferably, the Fe in the reaction raw material liquid 3+ The concentration is 0.5-1.2 mol / L, for example, it can be 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1.0 mol / L, 1.0 mol / L, 1.1 mol / L or 1.2 mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] In the present invention, when the iron-phosphorus ratio remains unchanged, Fe 3+ Changes in concentration will affect the particle size D50 and BET specific surface area of ​​the final ferric phosphate product. The particle size of ferric phosphate prepared within the concentration range of 0.5 to 1.2 mol / L meets the standard particle size requirements. Too high or too low a concentration will result in non-compliance with the standards.

[0019] Preferably, the phosphorus source comprises H3PO4.

[0020] Preferably, in the reaction raw material liquid, the molar ratio of iron to phosphorus is 0.9-1.5, for example, it can be 0.9, 1.0, 1.1, 1.2, 1.3, 1.4 or 1.5, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] Preferably, the reaction raw material liquid also includes a surfactant.

[0022] In the present invention, iron phosphate is precipitated in a low supersaturation environment and combined with a surfactant, which makes it easier to disperse particles and reduce agglomeration between particles, thereby facilitating the preparation of micro-nano iron phosphate with good crystallinity.

[0023] Preferably, the surfactant includes at least one of SDBS (sodium dodecylbenzene sulfonate), CTAB (cetyltrimethylammonium bromide), PEG-200 (polyethylene glycol-200), PEG-600 (polyethylene glycol-600) and PVA (polyvinyl alcohol), preferably a combination of PEG-600 and SDBS.

[0024] In the present invention, SDBS is an anionic surfactant, CTAB is a cationic surfactant, PEG-200, PEG-600 and PVA are nonionic surfactants, and PEG-200, PEG-600 and PVA are all polymers.

[0025] The nonionic surfactant PEG-600 combined with the ionic surfactant SDBS can achieve a synergistic effect. The critical micelle concentration of the mixed system is not equal to the average of the critical micelle concentrations of the two. The high molecular polymer PEG-600 has an adsorption effect on SDBS molecules through electrostatic attraction, which can reduce the number of free surfactant molecules, thereby increasing the critical micelle concentration of the surfactant and reducing the amount of surfactant used, making the required concentration of the compound surfactant lower than the concentration of using a single surfactant.

[0026] Preferably, based on the mass of the iron source, the mass fraction of the surfactant is 1 to 2.5%, for example, it can be 1%, 1.1%, 1.2%, 1.3%, 1.5%, 1.8%, 2%, 2.2% or 2.5%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] Preferably, the pH value of the reaction raw material liquid is 0.5-1, for example, it can be 0.5, 0.6, 0.7, 0.8, 0.9 or 1, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] In the present invention, the pH value of the reaction raw material liquid is controlled mainly to provide more H + ions, promoting the chemical balance in the positive direction, while avoiding Fe 3+ Ions and OH in solution - Ionic reaction generates Fe(OH)3 colloid, which prevents it from covering the surface of FePO4·2H2O and hindering the electrochemical performance. At the same time, when the pH value = 1, iron phosphate precipitation can begin to form. Controlling the pH value of the reaction raw material liquid can prevent precipitation from occurring due to the increase of pH value during storage. When the pH value of the reaction raw material liquid is too small or too large, the crystallinity of iron phosphate will be reduced.

[0029] Preferably, the flow rate of the reaction raw material liquid is 200-250 mL / min, for example, it can be 200 mL / min, 205 mL / min, 210 mL / min, 215 mL / min, 220 mL / min, 225 mL / min, 230 mL / min, 235 mL / min, 240 mL / min, 245 mL / min or 250 mL / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] Preferably, the pH adjuster comprises an alkaline solution.

[0031] Preferably, the alkaline solution comprises at least one of aqueous ammonia, sodium hydroxide solution, sodium carbonate solution and activated calcium oxide solution, preferably sodium hydroxide solution.

[0032] Taking Fe(NO3)3·9H2O and sodium hydroxide solution as an example, the equation for the precipitation reaction is:

[0033] Fe 3+ +3OH - =Fe(OH)3↓;

[0034] Fe(NO3)3+H3PO4+3NaOH=FePO4·2H2O↓+3NaNO3+H2O;

[0035] At this time, the product of the precipitation reaction is a yellow-brown mixture of FePO4 and Fe(OH)3.

[0036] Preferably, the solute mass concentration of the alkaline solution is 15-30%, for example, it can be 15%, 16%, 18%, 20%, 25%, 28% or 30%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] Preferably, the flow rate of the pH adjusting agent is 50 to 100 mL / min, for example, 50 mL / min, 55 mL / min, 60 mL / min, 65 mL / min, 70 mL / min, 75 mL / min, 80 mL / min, 85 mL / min, 90 mL / min, 95 mL / min or 100 mL / min, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0038] Preferably, the temperature of the precipitation reaction is 40-55°C, for example, it can be 40°C, 41°C, 42°C, 45°C, 48°C, 50°C, 52°C or 55°C; the time of the precipitation reaction is 1.0-3.0h, for example, it can be 1.0h, 1.1h, 1.2h, 1.5h, 1.8h, 2h, 2.2h, 2.5h, 2.8h or 3.0h; the pH value of the precipitation reaction is 1.5-2.5, for example, it can be 1.5, 1.6, 1.7, 1.8, 2, 2.2, 2.3 or 2.5, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0039] Preferably, the reagent used in the aging reaction includes a phosphoric acid solution, and the solute mass concentration of the phosphoric acid solution is 3 to 7%, for example, it can be 3%, 4%, 5%, 6% or 7%, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] The equation for the aging reaction is: Fe(OH)3+H3PO4=FePO4+3H2O.

[0041] Preferably, the temperature of the aging reaction is 85-95°C, for example, it can be 85°C, 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, 93°C or 94°C; the time of the aging reaction is 2-5h, for example, it can be 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] Preferably, the calcination temperature is 500-700°C, for example, it can be 500°C, 520°C, 550°C, 600°C, 650°C or 700°C; the calcination time is 2-4h, for example, it can be 2h, 2.5h, 3h, 3.5h or 4h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] As a preferred technical solution of the present invention, the method specifically comprises the following steps:

[0044] (I) dissolving an iron source in water, and then adding a phosphorus source to obtain a mixed solution; mixing the mixed solution with a surfactant to obtain a reaction raw material solution, wherein the pH value of the reaction raw material solution is 0.5 to 1;

[0045] (II) adding pure water as a bottom liquid into the reactor, and then simultaneously introducing the reaction raw material liquid and the pH adjusting agent into the pure water at the bottom of the reactor cavity, performing a precipitation reaction for 1.0 to 3.0 hours at a temperature of 40 to 55° C. and a pH value of 1.5 to 2.5, followed by separation, and then washing the separated solid product 1 to 3 times to obtain a ferric phosphate precursor; wherein the volume of the pure water is 10 to 20% (e.g., 10%, 12%, 15%, 18% or 20%) of the volume of the reactor; the pH adjusting agent includes an alkaline solution; the time for a single water washing is 30 to 60 minutes (e.g., 30 minutes, 40 minutes, 50 minutes or 60 minutes); during a single water washing, the volume ratio of the solid product to water is (3 to 6):1 (e.g., 3:1, 4:1, 5:1 or 6:1);

[0046] (III) adding the iron phosphate precursor to a phosphoric acid solution having a solute mass concentration of 3 to 7% according to a solid-liquid ratio of 1:(3 to 5) (e.g., 1:3, 1:4 or 1:5, etc.), performing an aging reaction at 85 to 95° C. for 2 to 5 hours, and then separating, and then washing the separated solid product with water for 1 to 3 times, and then drying at 100 to 120° C. for 2 to 4 hours to obtain iron phosphate dihydrate; wherein the time for a single water washing is 30 to 60 minutes (e.g., 30 minutes, 40 minutes, 50 minutes or 60 minutes, etc.); and the volume ratio of the solid product to water during the single water washing process is (3 to 6):1 (e.g., 3:1, 4:1, 5:1 or 6:1, etc.);

[0047] (IV) calcining the dihydrate iron phosphate at 500-700° C. for 2-4 hours to obtain the micro-nano iron phosphate.

[0048] In a second aspect, the present invention provides a micro-nano iron phosphate, which is prepared by the preparation method described in the first aspect.

[0049] Preferably, the particle size D50 of the micro-nano iron phosphate is 0.5-2 μm, for example, it can be 0.5 μm, 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 1.8 μm or 2 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0050] In a third aspect, the present invention provides a lithium iron phosphate positive electrode material, wherein raw materials for preparing the lithium iron phosphate positive electrode material include the micro-nano iron phosphate described in the second aspect and a lithium source.

[0051] Preferably, the preparation raw material also includes a carbon source.

[0052] In the present invention, when the raw materials include a carbon source, the obtained lithium iron phosphate positive electrode material includes a lithium iron phosphate core and a carbon layer coated on the surface of the core, which can improve the conductivity of the lithium iron phosphate positive electrode material.

[0053] Exemplarily, the method for preparing the lithium iron phosphate positive electrode material includes:

[0054] Micro-nano iron phosphate, a lithium source and a carbon source are mixed and sintered to obtain a lithium iron phosphate positive electrode material.

[0055] In a fourth aspect, the present invention provides a lithium-ion battery, wherein the positive electrode of the lithium-ion battery comprises the lithium iron phosphate positive electrode material described in the third aspect.

[0056] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0057] Compared with the prior art, the present invention has the following beneficial effects:

[0058] The present invention provides a method for continuously preparing micro-nano iron phosphate, wherein pure water is used as a base liquid, a co-precipitation environment with a low supersaturation concentration can be created, and a crystallization process can be better controlled; a reaction raw material liquid and a pH regulator are introduced simultaneously in order to cooperate with the pure water base liquid, the reaction raw material liquid and the pH regulator are introduced into the pure water at the same time, and precipitation is continuously generated in the pure water, and agglomeration of the generated precipitation can be avoided as much as possible, and the overall precipitation process is carried out in an environment with a low supersaturation concentration, which is conducive to the preparation of micro-nano iron phosphate with good crystallinity; compared with directly adding a pH regulator to the reaction raw material liquid, the method of adding the reaction raw material liquid and the pH regulator to the pure water at the same time can better control the binding rate of iron ions and phosphates in the precipitation process, avoid agglomeration of the formed iron phosphate, and thus improve the tap density of the final iron phosphate product;

[0059] The process of the present invention is a continuous process, which is easy to operate, environmentally friendly and economical. The prepared iron phosphate can reach the micro-nano level. 2+ The pre-oxidation step simplifies the process while saving acid and alkali, high raw material utilization, reduced costs, improved production efficiency and environmental protection. At the same time, the finished material has high purity, excellent performance, good product consistency, can be industrialized and easy to control automatically. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 A schematic flow chart of a method for continuously preparing micro-nano iron phosphate provided in an embodiment of the present invention.

[0061] Figure 2 and Figure 3 The SEM images of the micro-nano iron phosphate prepared in Example 1 of the present invention at different magnifications are shown.

[0062] Figure 4 This is the XRD diagram of the micro-nano iron phosphate prepared in Example 1 of the present invention.

[0063] Figure 5 This is the XRD diagram of the micro-nano iron phosphate prepared in Example 2 of the present invention.

[0064] Figure 6 This is the XRD diagram of the micro-nano iron phosphate prepared in Example 3 of the present invention.

[0065] Figure 7This is the XRD diagram of the micro-nano iron phosphate prepared in Example 4 of the present invention.

[0066] Figure 8 and Fig. 9 These are SEM images of the micro-nano iron phosphate prepared in Example 5 of the present invention at different magnifications.

[0067] Fig.10 and Fig.11 These are SEM images of the micro-nano iron phosphate prepared in Example 6 of the present invention at different magnifications.

[0068] Fig.12 and Fig.13 The SEM images of the micro-nano iron phosphate prepared in Comparative Example 1 of the present invention at different magnifications are shown. DETAILED DESCRIPTION

[0069] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0070] In one embodiment, the present invention provides a method for continuously preparing micro-nano iron phosphate, the process of which is as follows: Figure 1 As shown, the following steps are included:

[0071] A mixed solution of ferric nitrate, phosphoric acid and a surfactant is used as a reaction raw material liquid, the reaction raw material liquid and a pH regulator are simultaneously introduced into a pure water bottom liquid, a precipitation reaction is performed to precipitate ferric phosphate, the precipitated material is filtered to obtain a filtrate and a filter residue, and the filter residue is washed with water; the filter residue after washing is subjected to phosphoric acid aging, the solid product obtained by the phosphoric acid aging is washed with water and dried, and then the solid product is subjected to high-temperature calcination to obtain micro-nano ferric phosphate, wherein the micro-nano ferric phosphate is anhydrous ferric phosphate.

[0072] Example 1

[0073] This embodiment provides a method for continuously preparing micro-nano iron phosphate, comprising the following steps:

[0074] (1) dissolving Fe(NO3)3·9H2O in water, and then adding H3PO4 to obtain a mixed solution; mixing the mixed solution with a surfactant to obtain a reaction raw material solution, wherein Fe in the reaction raw material solution 3+ The concentration is 1.0 mol / L; the molar ratio of iron to phosphorus is 1.1; the surfactant is a mixture of PEG-600 and SDBS, the mass ratio of the two is 1:1, and the mass fraction of the surfactant is 1.5% based on the mass of the iron source; the pH value of the reaction raw material liquid is 0.8;

[0075] (2) adding pure water as a bottom liquid to the reactor, the volume of the pure water being 15% of the reactor volume, and then simultaneously introducing the reaction raw material liquid and the pH adjuster into the pure water at the bottom of the reactor cavity, the flow rate of the reaction raw material liquid being 230 mL / min, and the pH adjuster being a sodium hydroxide solution having a solute mass concentration of 20%, and the flow rate thereof being 50 mL / min; performing a precipitation reaction for 2.0 h at a temperature of 40° C. and a pH value of 2.1, followed by filtering, and then washing the filtered solid product three times with water to obtain an iron phosphate precursor; wherein the time for a single water washing is 30 min; and the volume ratio of the solid product to water during the single water washing process is 5:1;

[0076] (3) adding the iron phosphate precursor to a phosphoric acid solution with a solute mass concentration of 3% at a solid-liquid ratio of 1:5, performing an aging reaction at 90°C for 2 hours, and then filtering, and then washing the filtered solid product with water for 3 times, and then drying at 110°C for 3 hours to obtain iron phosphate dihydrate; wherein the time for a single water washing is 30 minutes; and the volume ratio of the solid product to water during the single water washing process is 5:1;

[0077] (4) calcining the dihydrate iron phosphate at 550° C. for 2 h to obtain micro-nano iron phosphate with a particle size D50 of 2 μm.

[0078] Figure 2 and Figure 3 The morphologies of the micro-nano iron phosphate prepared in Example 1 at 5k times and 5w times magnification are shown respectively. It can be seen from the figures that the micro-nano iron phosphate is formed into block particles through layer-by-layer accumulation of many smaller irregular rod-shaped structure particles. The large particles after secondary accumulation are evenly distributed without obvious agglomeration, and there are gaps between the particles.

[0079] Figure 4 The XRD diffraction results of the micro-nano iron phosphate prepared in Example 1 are shown. It can be seen from the figure that the spectrum of the finished micro-nano iron phosphate is basically consistent with the standard spectrum of hexagonal FePO4 (PDF#29-0715), the space group is P321 (150), the unit cell parameters are a=5.035nm, b=5.035nm, c=11.245nm, the characteristic peaks are also consistent, and the micro-nano iron phosphate has excellent crystallinity.

[0080] This embodiment also provides a method for preparing a lithium iron phosphate positive electrode material, comprising the following steps:

[0081] The prepared micro-nano iron phosphate, lithium hydroxide and glucose were mixed in a mass ratio of 7:2:1 and sintered at 700°C for 10 hours to obtain a lithium iron phosphate positive electrode material, which includes a lithium iron phosphate core and a carbon layer coated on the surface of the core.

[0082] Example 2

[0083] This embodiment provides a method for continuously preparing micro-nano iron phosphate, comprising the following steps:

[0084] (1) dissolving FeCl3·6H2O in water, and then adding H3PO4 to obtain a mixed solution; mixing the mixed solution with a surfactant to obtain a reaction raw material solution, wherein Fe in the reaction raw material solution 3+ The concentration is 1.0 mol / L; the molar ratio of iron to phosphorus is 1.1; the surfactant is CTAB, and the mass fraction of the surfactant is 1.5% based on the mass of the iron source; the pH value of the reaction raw material liquid is 0.8;

[0085] (2) adding pure water as a bottom liquid to the reactor, the volume of the pure water being 15% of the reactor volume, and then simultaneously introducing the reaction raw material liquid and the pH adjuster into the pure water at the bottom of the reactor cavity, the flow rate of the reaction raw material liquid being 230 mL / min, and the pH adjuster being a sodium hydroxide solution having a solute mass concentration of 20%, and the flow rate thereof being 50 mL / min; performing a precipitation reaction for 2.0 h at a temperature of 40° C. and a pH value of 2.1, followed by filtering, and then washing the filtered solid product three times with water to obtain an iron phosphate precursor; wherein the time for a single water washing is 30 min; and the volume ratio of the solid product to water during the single water washing process is 5:1;

[0086] (3) adding the iron phosphate precursor to a phosphoric acid solution with a solute mass concentration of 3% at a solid-liquid ratio of 1:5, performing an aging reaction at 90°C for 2 hours, and then filtering, and then washing the filtered solid product with water for 3 times, and then drying at 110°C for 2 hours to obtain iron phosphate dihydrate; wherein the time for a single water washing is 30 minutes; and the volume ratio of the solid product to water during the single water washing process is 5:1;

[0087] (4) calcining the dihydrate iron phosphate at 550° C. for 2 h to obtain micro-nano iron phosphate with a particle size D50 of 2 μm.

[0088] Figure 5 The XRD diffraction results of the micro-nano iron phosphate prepared in Example 2 are shown. It can be seen from the figure that the spectrum of the finished micro-nano iron phosphate is basically consistent with the standard spectrum of hexagonal FePO4 (PDF#29-0715), the space group is P321 (150), the unit cell parameters are a=5.035nm, b=5.035nm, c=11.245nm, the characteristic peaks are also consistent, and the micro-nano iron phosphate has excellent crystallinity.

[0089] This embodiment also provides a method for preparing a lithium iron phosphate positive electrode material, comprising the following steps:

[0090] The prepared micro-nano iron phosphate, lithium hydroxide and glucose were mixed in a mass ratio of 7:2:1 and sintered at 700°C for 10 hours to obtain a lithium iron phosphate positive electrode material, which includes a lithium iron phosphate core and a carbon layer coated on the surface of the core.

[0091] Example 3

[0092] The difference between this embodiment and embodiment 1 is that the pH value of the reaction raw material liquid is 0.2.

[0093] The remaining parameters remain the same as those in Example 1.

[0094] Figure 6 The XRD diffraction results of the micro-nano iron phosphate prepared in Example 3 are shown. Figure 6 and Figure 4 By comparison, it can be seen that compared with Example 1, the diffraction peak intensity of the characteristic peak at 25.822 of the micro-nano iron phosphate in this example is reduced, and the FWHM at this characteristic peak is increased; that is, when the pH value of the reaction raw material liquid is too small, the crystallinity of the iron phosphate will be reduced.

[0095] Example 4

[0096] The difference between this embodiment and embodiment 1 is that the pH value of the reaction raw material liquid is 1.2.

[0097] The remaining parameters remain the same as those in Example 1.

[0098] Figure 7 The XRD diffraction results of the micro-nano iron phosphate prepared in Example 4 are shown. It can be seen from the figure that compared with Example 1, the diffraction peak intensity of the characteristic peak at 25.822 of the micro-nano iron phosphate in this example decreases more significantly; that is, when the pH value of the reaction raw material liquid is too high, the crystallinity of the iron phosphate will be reduced.

[0099] Example 5

[0100] The difference between this embodiment and embodiment 1 is that no surfactant is added.

[0101] The remaining parameters remain the same as those in Example 1.

[0102] Figure 8 and Fig. 9The morphology of the micro-nano iron phosphate prepared in Example 5 at 5k times and 5w times magnification is shown in turn. It can be seen from the figure that the gap between the micro-nano iron phosphate is smaller, the rod-shaped structure particle shape and the layered structure are not obvious, and the large particles after secondary accumulation are agglomerated, and the particles are bonded together. The agglomeration and difficulty in dispersion of particles will inevitably lead to the inability of glucose to be evenly distributed on the surface of the iron phosphate particles during the preparation of lithium iron phosphate by mixing, so that the carbon layer cannot be effectively formed on the surface of the lithium iron phosphate core, resulting in poor conductivity of the lithium iron phosphate positive electrode material.

[0103] Example 6

[0104] The difference between this embodiment and embodiment 1 is that the surfactant is CTAB, and the mass fraction of the surfactant is 1.5%.

[0105] The remaining parameters remain the same as those in Example 1.

[0106] Fig.10 and Fig.11 The morphologies of the micro-nano iron phosphate prepared in Example 6 at 5k times and 5w times magnification are shown respectively. It can be seen from the figures that, compared with Example 1, many irregular rod-like structure particles are also stacked layer by layer to form block particles, but the rod-like structure begins to weaken, and the large particles after secondary stacking become more uneven in size, and there is also no obvious agglomeration phenomenon.

[0107] Comparative Example 1

[0108] The difference between this embodiment and embodiment 1 is that in step (2), the reaction raw material liquid is first introduced into the pure water for 30 minutes, and then the pH regulator is introduced.

[0109] The remaining parameters remain the same as those in Example 1.

[0110] Fig.12 and Fig.13 The morphologies of the micro-nano iron phosphate prepared in Comparative Example 1 at 5k times and 5w times magnification are shown in turn. It can be seen from the figure that the micro-nano iron phosphate in this comparative example precipitates at a relatively high saturation concentration, and the nucleation rate of the crystal nucleus is too fast, resulting in the inhibition of crystal growth, which leads to the agglomeration of crystal nuclei and amorphous precipitation. The agglomeration and difficulty in dispersion of particles will inevitably lead to the inability of glucose to be evenly distributed on the surface of the iron phosphate particles during the preparation of lithium iron phosphate by mixing, so that the carbon layer cannot be effectively formed on the surface of the lithium iron phosphate core, resulting in poor conductivity of the lithium iron phosphate positive electrode material.

[0111] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for continuously preparing micro-nano iron phosphate, characterized in that: The method comprises: The reaction raw material liquid and the pH regulator are simultaneously introduced into pure water to perform a precipitation reaction, and then an aging reaction and calcination are performed in sequence to obtain micro-nano iron phosphate; Wherein, the reaction raw material liquid includes an iron source and a phosphorus source.

2. The method for continuously preparing micro-nano iron phosphate according to claim 1, characterized in that: The iron source includes iron salts and / or iron oxides; Preferably, the iron salt includes at least one of Fe2(SO4)3, Fe(NO3)3 and FeCl3; the iron oxide includes Fe2O3; Preferably, the Fe in the reaction raw material liquid 3+ The concentration is 0.5~1.2mol / L; Preferably, the phosphorus source comprises H3PO4; Preferably, in the reaction raw material liquid, the molar ratio of iron element to phosphorus element is 0.9 to 1.

5.

3. The method for continuously preparing micro-nano iron phosphate according to claim 1 or 2, characterized in that: The reaction raw material liquid also includes a surfactant; Preferably, the surfactant comprises at least one of SDBS, CTAB, PEG-200, PEG-600 and PVA, preferably a combination of PEG-600 and SDBS; Preferably, based on the mass of the iron source, the mass fraction of the surfactant is 1 to 2.5%.

4. The method for continuously preparing micro-nano iron phosphate according to any one of claims 1 to 3, characterized in that: The pH value of the reaction raw material liquid is 0.5-1; Preferably, the flow rate of the reaction raw material liquid is 200-250 mL / min.

5. The method for continuously preparing micro-nano iron phosphate according to any one of claims 1 to 4, characterized in that: The pH adjuster includes an alkaline solution; Preferably, the alkaline solution includes at least one of aqueous ammonia, sodium hydroxide solution, sodium carbonate solution and activated calcium oxide solution; Preferably, the solute mass concentration of the alkaline solution is 15-30%; Preferably, the flow rate of the pH adjuster is 50-100 mL / min.

6. The method for continuously preparing micro-nano iron phosphate according to any one of claims 1 to 5, characterized in that: The temperature of the precipitation reaction is 40-55°C; the time of the precipitation reaction is 1.0-3.0h; the pH value of the precipitation reaction is 1.5-2.5; Preferably, the reagent used in the aging reaction includes a phosphoric acid solution, and the solute mass concentration of the phosphoric acid solution is 3-7%; Preferably, the temperature of the aging reaction is 85-95°C; the time of the aging reaction is 2-5h; Preferably, the calcination temperature is 500-700° C.; and the calcination time is 2-4 hours.

7. The method for continuously preparing micro-nano iron phosphate according to any one of claims 1 to 6, characterized in that: The method specifically comprises the following steps: (I) dissolving an iron source in water, and then adding a phosphorus source to obtain a mixed solution; mixing the mixed solution with a surfactant to obtain a reaction raw material solution, wherein the pH value of the reaction raw material solution is 0.5 to 1; (II) adding pure water as a bottom liquid into the reactor, and then simultaneously introducing the reaction raw material liquid and the pH adjusting agent into the pure water at the bottom of the reactor cavity, performing a precipitation reaction for 1.0 to 3.0 hours at a temperature of 40 to 55° C. and a pH value of 1.5 to 2.5, followed by separation, and then washing the separated solid product 1 to 3 times to obtain an iron phosphate precursor; wherein the volume of the pure water is 10 to 20% of the volume of the reactor; the pH adjusting agent includes an alkaline solution; the time for a single water washing is 30 to 60 minutes; and the volume ratio of the solid product to water during the single water washing is (3 to 6):1; (III) adding the iron phosphate precursor to a phosphoric acid solution having a solute mass concentration of 3 to 7% according to a solid-liquid ratio of 1:(3-5), performing an aging reaction at 85-95° C. for 2 to 5 hours, and then separating the separated solid product, washing it with water for 1 to 3 times, and then drying it at 100-120° C. for 2 to 4 hours to obtain iron phosphate dihydrate; wherein the time for a single water washing is 30 to 60 minutes; and the volume ratio of the solid product to water during the single water washing process is (3-6):1; (IV) calcining the dihydrate iron phosphate at 500-700° C. for 2-4 hours to obtain the micro-nano iron phosphate.

8. A micro-nano iron phosphate, characterized in that: The micro-nano iron phosphate is prepared by the preparation method according to any one of claims 1 to 7; Preferably, the particle size D50 of the micro-nano iron phosphate is 0.5-2 μm.

9. A lithium iron phosphate positive electrode material, characterized in that: The raw materials for preparing the lithium iron phosphate positive electrode material include the micro-nano iron phosphate described in claim 8 and a lithium source.

10. A lithium ion battery, characterized in that: The positive electrode of the lithium-ion battery includes the lithium iron phosphate positive electrode material according to claim 9.

Citation Information

Patent Citations

  • Preparation method of ferric phosphate with high tap density

    CN109721041A

  • Preparation method of spherical iron phosphate

    CN112624079A

  • Method for preparing lithium iron phosphate by doping metal elements in situ

    CN114702021A

  • Lithium manganese iron phosphate precursor as well as preparation method and application thereof

    CN117125690A

  • Preparation method for NANO ferric phosphate with low sulphur content

    WO2023273742A1

Cited By

  • Anhydrous iron phosphate and preparation method therefor, positive electrode material and preparation method therefor, positive electrode sheet, and secondary battery

    EP4793231A4