Molten salt dipping graphitization method for bamboo composite polymer-based waste

Through the low-temperature graphitization method of bamboo composite polymer-based waste in molten salt medium, the traditional high-temperature problem of graphitization is solved, simplified process and efficient graphitization are achieved, and it is suitable for the fields of conductive and thermally conductive materials.

CN119038541APending Publication Date: 2024-11-29ZHEJIANG JIAHE BAMBOO IND TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411165865.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The traditional graphitization process requires high temperatures, which limits its environmental protection and economic benefits. There are additional processes in existing low-temperature graphitization technology, which fails to simplify short-process processes.

Method used

After the bamboo composite polymer-based waste is powdered, amorphous carbon is formed by high temperature carbonization through inert atmosphere, and impregnation or direct carbonization is carried out in the molten salt medium to achieve low temperature graphitization, and the molten salt medium is used to provide the liquid phase environment to participate in the reaction.

Benefits of technology

It has achieved simplification of the process under low temperature conditions, improved graphitization efficiency, low cost and sustainable, and is suitable for the fields of conductive and thermally conductive materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038541A_ABST
    Figure CN119038541A_ABST
Patent Text Reader

Abstract

The invention discloses a molten salt impregnation graphitization method for bamboo composite polymer-based waste. The bamboo composite polymer-based waste is carbonized and subjected to molten salt dipping graphitization, or directly subjected to molten salt liquid medium carbonization graphitization, and finally the graphite is obtained after multiple times of cleaning. According to the method, the assistance of additional methods such as electrolysis, a catalyst and a reducing agent is not needed at the low temperature, and the fused salt is a liquid heat storage medium and a reactant and is suitable for all bamboo composite polymer-based waste materials. It shows that the introduced molten salt medium participating in the reaction can cooperate with thermal reduction to accelerate the graphitization reaction process of the bamboo wood composite polymer-based waste, and low-temperature impregnation and conversion of the molten salt into graphite are achieved. Besides, the method has the advantages of low cost, short process and efficient resource utilization of waste raw materials, and has wide application prospects in the field of waste graphitization of high-valued bamboo-wood composite polymer waste, plywood and the like, and the graphite product also has high commercial value in the fields of lithium battery negative electrodes, electric conduction and heat conduction materials and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for graphitizing bamboo composite polymer-based waste by molten salt impregnation, in particular to a method for converting bamboo waste into artificial graphite at low temperature, belonging to the field of high-value conversion of bamboo waste into carbon nanomaterials. Background Art

[0002] Graphite has been widely used in many fields such as electrode materials, thermal conductive materials and conductive plates due to its excellent electrical and thermal conductivity. Nevertheless, natural graphite is limited in supply, and its application faces challenges due to its unstable quality and the negative impact of mining activities on the environment. In this regard, synthetic graphite has the advantages of its abundant sources, low cost and sustainability, especially the conversion of waste biomass materials into graphite. However, the traditional graphitization process needs to be carried out at temperatures as high as 3000°C, which limits its environmental and economic benefits. Recently, the development of molten salt low-temperature graphitization technology has effectively reduced the processing temperature to below 1000°C, greatly enhancing the application range and practicality of synthetic graphite.

[0003] Patent CN103510103 describes an electrochemical low-temperature graphitization method that can convert amorphous carbon into graphite at 700°C by means of electrolysis. In addition, another patent CN12442761A introduces a method for converting amorphous carbon into graphitized carbon nanofibers at 600°C by introducing transition metal compounds. However, these technologies all involve additional steps, such as the use of catalysts or electronic assistance, and thus fail to achieve a short-process graphitization process. These limitations indicate that there is room for further research and development to promote the simplification and efficiency of graphitization technology.

[0004] In addition, treating composite polymer-based waste as a renewable biomass resource has significant advantages, including low cost. Therefore, converting such waste into graphite is not only important for realizing its high-value application, but also promotes the recycling of resources and reduces the burden of waste on the environment. Summary of the invention

[0005] In view of the shortcomings of the above-mentioned technology, the present invention provides a method for graphitizing bamboo composite polymer-based waste by molten salt impregnation.

[0006] The solution adopted by the present invention to solve the above technical problems is:

[0007] ① Powdering the bamboo composite polymer-based waste, the material treatment sequence after pulverization is firstly carbonizing in an inert atmosphere at high temperature to form amorphous carbon, and then introducing molten salt medium for impregnation to achieve graphitization;

[0008] or,

[0009] ② The bamboo composite polymer-based waste is pulverized, and the pulverized material is introduced into a molten salt medium for carbonization, and a graphitization process is carried out at the same time.

[0010] The molten salt not only provides a high-temperature liquid environment, but also participates in activation and graphitization or carbonization reactions. After the reaction is completed, graphite is obtained after cooling and cleaning.

[0011] The bamboo composite polymer-based waste material of the present invention is a mixture of bamboo and polymer. The bamboo material in the bamboo composite polymer-based waste material is selected from at least one of light bamboo waste, giant dragon bamboo waste, tea bamboo waste, arrow bamboo waste, ci bamboo waste, and moso bamboo waste, or a mixture thereof, and the polymer is selected from at least one of phenolic resin, urea-formaldehyde resin, melamine resin, epoxy resin, polyurethane resin, amino resin, polyester resin, polyether resin, and nitro resin, or a mixture thereof, wherein the mass percentage of the polymer in the whole waste material is 0.1% to 55%.

[0012] In scheme ①, the carbonization temperature is generally 500-1000°C, and the carbonization time is generally 2-24h.

[0013] In scheme ①, the amorphous carbon formed by carbonization is activated, impurity-removed and graphitized in molten salt.

[0014] In scheme ②, the waste is carbonized, activated, decontaminated and graphitized in molten salt.

[0015] Preferably, during the molten salt treatment process, the upper gas phase of the molten salt is an inert gas.

[0016] The above-mentioned carbonization in molten salt means that bamboo composite polymer-based waste is directly added to the molten salt medium for carbonization pyrolysis. The above-mentioned molten salt activation / impurity removal means that the bamboo composite polymer-based waste derived carbon and impurities can spontaneously react with the molten salt medium to achieve activation (1 to 24 hours) / impurity removal (1 to 24 hours) treatment, and the reaction products can be removed by washing.

[0017] Preferably, in scheme ①, the amorphous carbon needs to be ball-milled and then placed in molten salt for treatment, and the ball-milling time is 2 to 24 hours.

[0018] Preferably, the molten salt is a molten electrolyte, and its anion is SO3 2- 、SO4 2- 、CO3 2- 、NO3 - , Cl - 、F - At least two of the following; the cation is Li + , K + 、Na + , Ca 2+ 、Al 3+ , Fe3+ One or more of the following; the working temperature of the molten salt is 200~1000℃.

[0019] Preferably, under molten salt impregnation graphitization, the impregnation time is 2 to 24 hours.

[0020] Preferably, the prepared graphite presents a lamellar bulk structure with a length of about 500nm to 5μm.

[0021] The graphite process prepared by the present invention is different from the graphite preparation method of its patent CN103510103 and patent CN112442761 A. In order to simplify the experimental process and improve the graphitization efficiency, the present invention immerses the bamboo composite polymer-based waste in a special combination of molten salt media to achieve its graphitization through interaction, and its graphitization degree is comparable to that reported (Angew. Chem. Int. Ed. Engl. 2017, 56, 1751). This shows that the interaction between the bamboo composite polymer-based waste and the molten salt of suitable components is very beneficial to the graphitization process.

[0022] The present invention adopts an innovative method to immerse bamboo composite polymer-based waste in a molten salt medium, and realize low-temperature graphitization through the interaction between the medium and the material. This method is not only low-cost and short in process, but also sustainable, and provides an effective way to derive carbonaceous materials from bamboo waste under low-temperature conditions. This technology has shown significant commercial potential in the fields of conductive and thermal conductive materials, energy storage materials, etc., and indicates a wide range of application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The SEM and XRD images of the moso bamboo composite polymer-based waste before and after graphitization in Example 1 show that the product is graphite;

[0024] Figure 2 is a SEM image of the product of Example 2, showing graphite;

[0025] Figure 3 is a SEM image of the product of Example 6, showing graphite;

[0026] Figure 4 is a SEM image of the product of Example 7, showing graphite;

[0027] Figure 5 is a SEM image of the product of Example 8, showing graphite;

[0028] Figure 6 The SEM images of the product of Example 12 and the product of Comparative Example 1 show that Comparative Example 1 is amorphous carbon, and the product of Example 12 is graphite. DETAILED DESCRIPTION

[0029] The following paragraphs elaborate on specific embodiments of the present invention, which are intended to help professionals in the field of this technology better understand and implement the present invention. Although this document describes specific implementations in detail, it should be emphasized that the scope of the present invention is not limited to these examples. For ordinary technicians in this technical field, any obvious changes and adjustments within the spirit and scope of the present invention as defined by the attached claims should be deemed to be within the scope of protection of the present invention. Therefore, all innovative applications of the present invention based on original ideas are protected by law.

[0030] The present invention provides a first typical solution: bamboo composite polymer-based waste is first carbonized at high temperature in an inert atmosphere, introduced into a molten salt medium for immersion after ball milling, washed with hydrochloric acid, water, etc. after the immersion, and finally dried and stored.

[0031] The present invention provides a second typical solution: bamboo composite polymer-based waste is directly introduced into molten salt for carbonization and impregnation, and after the impregnation, it is cleaned with hydrochloric acid, water, etc., and finally dried and stored.

[0032] Example 1

[0033] The bamboo composite polymer-based waste (99wt% bamboo waste + 1% epoxy resin) was carbonized at 800℃ for 4h, then ball-milled for 10h, and 5g was immersed in 850℃ Na2CO3-NaCl-LiCl molten salt (molar ratio 1:1:1) electrolyte for 10h. After the immersion, the product was rinsed with water, 0.1M hydrochloric acid and acetone, and finally dried and stored at 80℃. XRD and SEM tests showed that the bamboo composite polymer-based waste had been converted into graphite, such as Figure 1 shown.

[0034] Example 2

[0035] The light bamboo composite polymer-based waste (99.9wt% light bamboo waste + 0.1% urea-formaldehyde resin) was carbonized at 600℃ for 4h, then ball-milled for 10h, and 5g was immersed in 850℃ Na2CO3-NaCl-KCl molten salt (molar ratio 2:1:1) electrolyte for 12h. After the immersion, the product was rinsed with water, 0.1M hydrochloric acid and acetone, and finally dried and stored at 80℃. The test showed that the light bamboo composite polymer-based waste had been converted into graphite, such as Figure 2 shown.

[0036] Example 3

[0037] The composite polymer-based waste of arrow bamboo (45wt% arrow bamboo waste + 55% phenolic resin) was carbonized at 1000℃ for 2h, then ball-milled for 10h, and 5g was immersed in 800℃ Na2CO3-NaCl-CaCl2 molten salt (molar ratio 2:1:1) electrolyte for 8h. After the immersion, the product was rinsed with water, 0.1M hydrochloric acid and acetone, and finally dried and stored at 80℃. The test showed that the composite polymer-based waste of arrow bamboo had been converted into graphite.

[0038] Example 4

[0039] The composite polymer-based waste of giant dragon bamboo (55wt% arrow bamboo waste + 45% phenolic resin) was carbonized at 500℃ for 24h, then ball-milled for 10h, and 5g was immersed in 800℃ NaF-NaCl-AlCl3 molten salt (molar ratio 4:1:1) electrolyte for 6h. After the immersion, the product was rinsed with water, 0.1M hydrochloric acid and acetone, and finally dried and stored at 80℃. The test showed that the composite polymer-based waste of giant dragon bamboo had been converted into graphite.

[0040] Example 5

[0041] The bamboo composite polymer-based waste (95wt% bamboo waste + 5% amino resin) was carbonized at 800℃ for 4h, then ball-milled for 10h, and 5g was immersed in 850℃ NaNO3-NaCl-CaCl2 molten salt (molar ratio 2:1:1) electrolyte for 8h. After the immersion, the product was rinsed with water, 0.1M hydrochloric acid and acetone, and finally dried and stored at 80℃. The test showed that the bamboo composite polymer-based waste had been converted into graphite.

[0042] Example 6

[0043] The light bamboo composite polymer-based waste (75wt% light bamboo waste + 25% nitro resin) was carbonized at 850℃ for 4h, then ball-milled for 10h, and 5g was immersed in 800℃ NaNO3-NaCl-KCl molten salt (molar ratio 2:1:1) electrolyte for 10h. After the immersion, the product was rinsed with water, 0.1M hydrochloric acid and acetone, and finally dried and stored at 80℃. The test showed that the light bamboo composite polymer-based waste had been converted into graphite, such as Figure 3 shown.

[0044] Example 7

[0045] Take 10g of bamboo composite polymer waste (55wt% bamboo waste + 45% phenolic resin) and immerse it in 850℃ Na2CO3-NaCl-LiCl molten salt (molar ratio 2:1:1) electrolyte for 12h. After immersion, the product is washed with water, 0.1M hydrochloric acid and acetone, and finally dried and stored at 80℃. Tests show that bamboo composite polymer waste has been converted into graphite, such as Figure 4 shown.

[0046] Example 8

[0047] Take 10g of Julong bamboo composite polymer-based waste (75wt% Julong bamboo waste + 25% polyether resin) and immerse it in 850℃ Na2CO3-NaCl-KCl molten salt (molar ratio 2:1:1) electrolyte for 14h. After the immersion, the product was washed with water, 0.1M hydrochloric acid and acetone, and finally dried and stored at 80℃. The test showed that the Julong bamboo composite polymer-based waste has been converted into graphite, such as Figure 5 shown.

[0048] Example 9

[0049] Take 10g of bamboo composite polymer waste (75wt% bamboo waste + 25% phenolic resin) and immerse it in 800℃ Na2CO3-NaCl-CaCl2 molten salt (molar ratio 2:1:1) electrolyte for 10h. After immersion, the product is washed with water, 0.1M hydrochloric acid and acetone, and finally dried and stored at 80℃. Tests show that bamboo composite polymer waste has been converted into graphite.

[0050] Example 10

[0051] Take 10g of light bamboo composite polymer-based waste (85wt% light bamboo waste + 15% phenolic resin) and immerse it in 800℃ NaF-NaCl-AlCl3 molten salt (molar ratio 2:1:1) electrolyte for 8h. After immersion, the product is washed with water, 0.1M hydrochloric acid and acetone, and finally dried and stored at 80℃. The test shows that the light bamboo composite polymer-based waste has been converted into graphite.

[0052] Embodiment 11

[0053] Take 10g of bamboo composite polymer waste (75wt% bamboo waste + 25% phenolic resin) and immerse it in 850℃ NaNO3-NaCl-CaCl2 molten salt (molar ratio 3:1:1) electrolyte for 10h. After immersion, the product is washed with water, 0.1M hydrochloric acid and acetone, and finally dried and stored at 80℃. Tests show that bamboo composite polymer waste has been converted into graphite.

[0054] Example 12

[0055] Take 10g of Julong bamboo composite polymer-based waste (55wt% Julong bamboo waste + 45% phenolic resin) and immerse it in 800℃ NaNO3-NaCl-KCl (molar ratio 2:1:1) molten salt electrolyte for 12h. After immersion, the product was washed with water, 0.1M hydrochloric acid and acetone, and finally dried and stored at 80℃. The test showed that the Julong bamboo composite polymer-based waste has been converted into graphite, such as Figure 6 shown.

[0056] Comparative Example 1

[0057] Take 10g of Julong bamboo composite polymer-based waste (55wt% Julong bamboo waste + 45% phenolic resin) and immerse it in 800℃ NaCl-KCl molten salt (molar ratio 1:1) electrolyte for 12h. After the immersion, the product was washed with water, 0.1M hydrochloric acid and acetone, and finally dried and stored at 80℃. The test showed that the Julong bamboo composite polymer-based waste was not converted into graphite.

[0058] Comparative Example 2

[0059] Take 10g of Julong bamboo composite polymer-based waste (55wt% Julong bamboo waste + 45% phenolic resin) and immerse it in 800℃ NaNO3-KNO3-Ca(NO3)2 molten salt (molar ratio 1:1:1) electrolyte for 12h. After the immersion, the product was washed with water, 0.1M hydrochloric acid and acetone, and finally dried and stored at 80℃. The test showed that the Julong bamboo composite polymer-based waste was not converted into graphite.

[0060] Finally, it should be pointed out that the above specific implementation is mainly used to illustrate the technical content of the present invention and does not constitute a limitation of the present invention. Although the present invention has been described in detail through specific examples, it should be understood by those skilled in the art that the technical solution of the present invention can also be modified or replaced by equivalents, and these modifications or replacements should not deviate from the core spirit and scope of the technical solution of the present invention. All these changes, modifications and equivalent replacements within the spirit and principle of the technical solution should be included in the scope of protection of the claims of the present invention.

Claims

1. A method for graphitizing bamboo composite polymer-based waste by molten salt impregnation, characterized in that: The following steps are involved: The bamboo composite polymer-based waste is first carbonized at high temperature in an inert atmosphere to form amorphous carbon, and then introduced into a molten salt medium for impregnation to achieve graphitization. Alternatively, the bamboo composite polymer-based waste can be directly introduced into a molten salt medium for immersion, thereby achieving carbonization and graphitization. After the reaction is completed, graphite can be obtained after cooling and washing.

2. The method for graphitizing bamboo composite polymer-based waste by molten salt impregnation according to claim 1, characterized in that: The bamboo composite polymer-based waste is a mixture, and the mixture is a mixture of bamboo and polymer; wherein the mass percentage of the polymer in the whole waste is 0.1% to 55%.

3. The method for graphitizing bamboo composite polymer-based waste by molten salt impregnation according to claim 2, characterized in that: The bamboo material in the bamboo composite polymer-based waste is selected from at least one of light bamboo waste, giant dragon bamboo waste, tea bamboo waste, arrow bamboo waste, citrus bamboo waste, and moso bamboo waste, or a mixture thereof.

4. The method for graphitizing bamboo composite polymer-based waste by molten salt impregnation according to claim 2, characterized in that: The high molecule in the bamboo composite high molecule-based waste is a polymer, and the high molecule is selected from at least one of phenolic resin, urea-formaldehyde resin, melamine resin, epoxy resin, polyurethane resin, amino resin, polyester resin, polyether resin, and nitro resin, or a mixture thereof.

5. The method for graphitizing bamboo composite polymer-based waste by molten salt impregnation according to claim 1, characterized in that: The upper gas phase of the molten salt medium is an inert gas.

6. The method for graphitizing bamboo composite polymer-based waste by molten salt impregnation according to claim 1, characterized in that: The temperature of high temperature carbonization is 500-1000°C, and the carbonization time is 2-24h.

7. The method for graphitizing bamboo composite polymer-based waste by molten salt impregnation according to claim 1, characterized in that: The amorphous carbon is immersed in a molten salt medium after ball milling, and the ball milling time is 2 to 24 hours.

8. The method for graphitizing bamboo composite polymer-based waste by molten salt impregnation according to claim 1, characterized in that: The molten salt is an electrolyte, and its anion is SO3 2- 、SO4 2- 、CO3 2- 、NO3 - , Cl - 、F - At least two of the following; the cation is Li + , K + 、Na + , Ca 2+ 、Al 3+ , Fe 3+ One or more of the following; the working temperature of the molten salt is 200~1000℃.

9. The method for graphitizing bamboo composite polymer-based waste by molten salt impregnation according to claim 1, characterized in that: The immersion time is 2 to 24 hours.

Citation Information

Patent Citations

  • CH561751A5

  • Method for converting amorphous carbon to graphitized carbon nanofibers

    CN112442761A

  • Method for preparing porous carbon for super capacitor by waste plastic carbonization

    CN105366658A

  • Biomass three-dimensional porous graphene and preparation method thereof

    CN111547709A

  • Method for preparing three-dimensional porous graphene sheet by adopting low-temperature double-salt compound and application of three-dimensional porous graphene sheet