Preparation method of lithium cobalt oxide, application of lithium cobalt oxide in preparation of electrode and battery

The lithium cobalt oxide powder prepared by one-step sintering method is applied to lithium battery electrodes, solving the problems of complex preparation and poor performance of LiCoO2 particles in the prior art, and achieving high bulk density and high voltage lithium battery performance, especially at 4.5V The gram capacity of lithium batteries under the voltage platform has been significantly improved.

CN119038622APending Publication Date: 2024-11-29WUHU ETC BATTERY LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411274683.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art requires multiple processes and difficult-to-control factors when preparing LiCoO2 particles, resulting in the problem of rapid decay of their capacity during the cycle, especially in the condition of 4.5V or above, which is difficult to achieve satisfactory performance.

Method used

Precursor liquid is prepared by a mixture of ethylene glycol methyl ether and monoethanolamine. Through a one-step sintering method, the reaction temperature and time are controlled, and LiCoO2 particles with smooth surface and excellent high voltage performance are prepared, and applied to the electrode to improve lithium Battery bulk density and voltage performance.

Benefits of technology

The application of lithium cobalt oxide powder prepared by one-step sintering method in electrodes has significantly improved the surface morphology and size distribution of LiCoO2 particles, reduced particle fracture, improved lithium ion diffusion ability, and achieved high bulk density and high voltage. The performance of lithium batteries, especially under the 4.5V voltage platform, the gram capacity of lithium batteries can reach more than 190mAh/g.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038622A_ABST
    Figure CN119038622A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of lithium cobalt oxide, application of the lithium cobalt oxide in preparation of an electrode and a battery. The preparation method of the lithium cobalt oxide comprises the following steps: adding a lithium salt, a cobalt salt and an organic acid into a mixed solution of ethylene glycol monomethyl ether and monoethanolamine to obtain a precursor solution; and calcining the precursor solution to obtain the lithium cobalt oxide. The prepared lithium cobalt oxide powder is applied to preparation of an electrode, and the prepared electrode is used for further preparing a button battery. The precursor solution is prepared from the mixed solution of ethylene glycol monomethyl ether and monoethanolamine in a proper ratio, the surface morphology of LiCoO2 particles can be improved through one-step sintering at a proper temperature, the surface morphology of cathode particles becomes neat and smooth, uniform lithium diffusion is ensured, generation of local strain is relieved, particle breakage is reduced, and the performance of the lithium ion battery is improved. The lithium ion diffusivity is improved, and the possibility is provided for realizing a lithium battery with high stacking density and high voltage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the preparation and application of a lithium battery cathode material, and in particular to a preparation method of lithium cobalt oxide and the application of the lithium cobalt oxide in the preparation of electrodes and a battery. Background Art

[0002] LiCoO 2 Due to its high packing density, high operating voltage and excellent cycle stability, it is considered the most successful cathode material in portable electronics. The energy density of a battery is highly correlated with its specific capacity and voltage window. However, under the condition of 4.2V, LiCoO 2 To a certain extent, only about half of its theoretical capacity can be released. Therefore, in order to improve LiCoO 2 To solve the problem of rapid capacity decay during cycling, LiCoO with satisfactory performance above 4.5 V was synthesized. 2 The material remains somewhat challenging.

[0003] At present, common preparation methods include hydrothermal method, microwave method, solid phase synthesis method, etc., but they all require the synthesis of precursors first, and then the formation of LiCoO through secondary sintering. 2 particles, more processes, and more difficult-to-control factors, which affect the LiCoO 2 Final performance trends. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to provide a method for preparing lithium cobalt oxide, which solves the problem of how to prepare LiCoO by one-time sintering. 2 Another object of the present invention is to propose an application of lithium cobalt oxide powder prepared by the above preparation method in the preparation of electrodes, so as to solve the problem of how to use lithium cobalt oxide powder to prepare electrodes. The third object of the present invention is to propose a battery with high packing density and high voltage comprising the above electrode.

[0005] Technical solution: A method for preparing lithium cobalt oxide according to the present invention comprises the following steps:

[0006] (1) adding lithium salt, cobalt salt and organic acid to a mixture of ethylene glycol methyl ether and monoethanolamine to obtain a precursor solution;

[0007] (2) Calcinate the precursor solution to obtain lithium cobalt oxide.

[0008] The present invention uses a mixed solution of ethylene glycol methyl ether and monoethanolamine to prepare a precursor solution, so that ions in the solution are stably and evenly distributed in the solvent, and through one-step sintering, the reaction temperature and time are controlled to prepare an LCO particle material with a smooth surface and excellent high voltage performance.

[0009] Preferably, in step (1), the volume ratio of ethylene glycol methyl ether to monoethanolamine in the mixed solution of ethylene glycol methyl ether and monoethanolamine is 5-15:1.

[0010] Preferably, in step (1), the lithium salt includes at least one of lithium acetate, lithium phosphate, lithium carbonate, lithium chloride, lithium sulfate and lithium nitrate; the cobalt salt includes at least one of cobalt nitrate, cobalt carbonate, cobalt sulfate and cobalt chloride; and the organic acid includes at least one of citric acid, malic acid, acetic acid, formic acid and oxalic acid.

[0011] Preferably, in step (1), the molar ratio of the lithium salt, the cobalt salt and the organic acid is 1-3:0.5-1.5:1-2.5.

[0012] Preferably, in step (1), the mass ratio of the total weight of the lithium salt, the cobalt salt and the organic acid to the mixed solution of ethylene glycol methyl ether and monoethanolamine is 1-10:2-100.

[0013] Preferably, in step (2), the calcination method is: in an air environment, heating to 750-850° C. at a rate of 1-3° C. / min, and sintering at this temperature for 6-24 hours.

[0014] The present invention further uses the lithium cobalt oxide powder prepared by the above preparation method in preparing electrodes.

[0015] The method for preparing an electrode using the above-mentioned lithium cobalt oxide powder comprises the following steps:

[0016] (1) adding the lithium cobalt oxide powder obtained by the preparation method according to any one of claims 1 to 6, a conductive agent and a binder into N-methylpyrrolidone and mixing them thoroughly to obtain a slurry;

[0017] (2) The slurry is coated on a substrate, vacuum dried, and then rolled to obtain an electrode.

[0018] Preferably, the conductive agent is selected from at least one of acetylene black, graphite and carbon black; the binder is selected from at least one of polyvinylidene fluoride, polytetrafluoroethylene and sodium carboxymethyl cellulose; and the substrate is selected from at least one of aluminum foil, copper foil, carbon cloth and carbon paper.

[0019] Based on the above electrode, the present invention further discloses a battery comprising the above electrode.

[0020] In some embodiments, the button cell was assembled in an argon-filled glove box, using lithium metal foil as the counter electrode and polypropylene film (Celgard 2400) as the separator. 6 The salt was dissolved in a mixed solution of ethyl carbonate (EC) and dimethyl carbonate (DMC) with a volume ratio of 1:1 as the electrolyte, and LiPF 6 The salt concentration is 1 mol / L.

[0021] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:

[0022] 1. The present invention uses a mixture of ethylene glycol methyl ether and monoethanolamine in an appropriate ratio to prepare a precursor solution, and a one-step sintering at an appropriate temperature can improve the LiCoO 2 The surface morphology of the particles and the surface morphology of the cathode particles become neat and smooth, ensuring uniform lithium diffusion, thereby alleviating the generation of local strain, thereby reducing particle breakage, improving lithium ion diffusion capacity, and providing the possibility of achieving high stacking density and high voltage lithium batteries.

[0023] 2. The present invention can improve LiCoO 2 The particle size of the particles increases the packing density of the material and reduces agglomeration caused by irregular material size.

[0024] 3. The present invention changes LiCoO 2 The morphology and size of the particles reduce the large number of blank sites between the particles, reduce the fluidity of the particles, and achieve high stacking density and high voltage lithium batteries. When used on a 4.5V voltage platform, the gram capacity can reach more than 190mAh / g. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 LiCoO prepared in Example 1 2 SEM images of particles;

[0026] Figure 2 LiCoO prepared in Example 2 2 SEM images of particles;

[0027] Figure 3 LiCoO prepared in Example 3 2 SEM images of particles;

[0028] Figure 4 LiCoO prepared in Example 4 2 SEM images of particles;

[0029] Figure 5 LiCoO prepared in Example 5 2 SEM images of particles;

[0030] Figure 6 LiCoO prepared in Example 6 2 SEM images of particles;

[0031] Figure 7 LiCoO prepared in Comparative Example 1 2 SEM images of particles;

[0032] Figure 8 LiCoO prepared in Comparative Example 2 2 SEM images of particles;

[0033] Fig. 9 LiCoO prepared in Comparative Example 3 2 SEM images of particles;

[0034] Fig.10 LiCoO prepared in Comparative Example 4 2 SEM images of particles;

[0035] Fig.11 LiCoO prepared in Comparative Example 5 2 SEM images of particles;

[0036] Fig.12 For the use of different LiCoO 2 Performance diagram of the particle button battery;

[0037] Fig.13 For the use of different LiCoO 2 dQ-dV data graph of the button battery with particles. DETAILED DESCRIPTION

[0038] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0039] Embodiment 1: A method for preparing lithium cobalt oxide, comprising the following steps:

[0040] (1) mixing ethylene glycol methyl ether and monoethanolamine in a volume ratio of 10:1 to obtain a mixed solution;

[0041] (2) lithium acetate, cobalt nitrate and citric acid monohydrate are added to the mixed solution of step (1) in sequence on a hot plate at 50° C., and stirred for 12 hours to obtain a precursor solution; the molar ratio of lithium acetate, cobalt nitrate and citric acid monohydrate is 2:1:1.8; and the mass ratio of the total weight of the lithium acetate, cobalt nitrate and citric acid monohydrate to the mixed solution is 1:5.

[0042] (3) The precursor liquid is transferred to a porcelain boat, each porcelain boat is filled with 3-5 mL of the precursor liquid, and the porcelain boat is placed in a muffle furnace. In an air environment, the temperature is increased to 800°C at 2°C / min, and the temperature is kept for sintering for 12 hours.

[0043] (4) Take out the solid powder after sintering and put it in an air flow pulverizer for pulverization and grinding. The black powder obtained is lithium cobalt oxide particles. Figure 1 As shown, the surface morphology of lithium cobalt oxide particles is neat and smooth.

[0044] Embodiment 2: A method for preparing lithium cobalt oxide, comprising the following steps:

[0045] (1) mixing ethylene glycol methyl ether and monoethanolamine in a volume ratio of 10:1 to obtain a mixed solution;

[0046] (2) lithium phosphate, cobalt carbonate and malic acid are added to the mixed solution in sequence on a hot plate at 50° C., and stirred for 8 hours to obtain a precursor solution; the molar ratio of lithium phosphate, cobalt carbonate and malic acid is 1:0.5:1; and the mass ratio of the total weight of the lithium phosphate, cobalt carbonate and malic acid to the mixed solution is 1:2.

[0047] (3) The precursor liquid is transferred to a porcelain boat, each porcelain boat is filled with 3-5 mL of the precursor liquid, and the porcelain boat is placed in a muffle furnace. In an air environment, the temperature is increased to 850°C at 1°C / min and sintered for 12 hours.

[0048] (4) Take out the solid powder after sintering and put it in an air flow pulverizer for pulverization and grinding. The black powder finally obtained is lithium cobalt oxide particles, such as Figure 2 As shown, the surface morphology of lithium cobalt oxide is relatively smooth.

[0049] Embodiment 3: A method for preparing lithium cobalt oxide, comprising the following steps:

[0050] (1) mixing ethylene glycol methyl ether and monoethanolamine in a volume ratio of 10:1 to obtain a mixed solution;

[0051] (2) lithium carbonate, cobalt sulfate and oxalic acid are added to the mixed solution in sequence on a hot plate at 50° C., and stirred for 24 hours to obtain a precursor solution; the molar ratio of lithium carbonate, cobalt sulfate and oxalic acid is 3:1.5:2.5; and the mass ratio of the total weight of the lithium carbonate, cobalt sulfate and oxalic acid to the mixed solution is 1:10.

[0052] (3) The precursor liquid is transferred to a porcelain boat, each porcelain boat is filled with 3-5 mL of the precursor liquid, and the porcelain boat is placed in a muffle furnace. In an air environment, the temperature is increased to 750°C at 3°C / min, and the temperature is kept for sintering for 24 hours.

[0053] (4) Take out the solid powder after sintering and put it in an air flow pulverizer for pulverization and grinding. The black powder finally obtained is lithium cobalt oxide particles, such as Figure 3 As shown, edges appear on the surface of lithium cobalt oxide, but the overall morphology is uniform and of uniform size.

[0054] Embodiment 4: The rest is the same as Embodiment 1, except that:

[0055] In step (2), lithium acetate is replaced by lithium chloride; cobalt nitrate is replaced by cobalt chloride; citric acid monohydrate is replaced by acetic acid

[0056] In step (3), the sintering is carried out for 6 hours.

[0057] The morphology of the lithium cobalt oxide particles prepared in this embodiment is as follows: Figure 4As shown, the surface of lithium cobalt oxide is smooth, the particle size is small and easy to agglomerate.

[0058] Embodiment 5: The rest is the same as Embodiment 1, except that:

[0059] In step (2), lithium acetate is replaced by lithium sulfate; citric acid monohydrate is replaced by formic acid. The powder finally obtained is lithium cobalt oxide particles.

[0060] The morphology of the lithium cobalt oxide particles prepared in this embodiment is as follows: Figure 5 As shown, there are a few cracks on the surface of lithium cobalt oxide.

[0061] Embodiment 6: The rest is the same as Embodiment 1, except that:

[0062] In step (2), lithium acetate is replaced by lithium nitrate; cobalt nitrate is replaced by cobalt chloride. The powder finally obtained is lithium cobalt oxide particles.

[0063] The morphology of the lithium cobalt oxide particles prepared in this embodiment is as follows: Figure 6 As shown, the surface of lithium cobalt oxide is smooth and there are protrusions on the surface of the sphere.

[0064] Comparative Example 1: The rest is the same as Example 1, except that:

[0065] Ethylene glycol methyl ether was used to replace monoethanolamine, that is, only ethylene glycol methyl ether, lithium acetate, cobalt nitrate and citric acid monohydrate were used to prepare the precursor solution.

[0066] The morphology of the lithium cobalt oxide particles prepared in this comparative example is as follows Figure 7 As shown, the lithium cobalt oxide spheres are uneven in size and have a rough surface.

[0067] Comparative Example 2: The rest is the same as Example 1, except that:

[0068] The volume ratio of ethylene glycol methyl ether to monoethanolamine is 5:1.

[0069] The morphology of the lithium cobalt oxide particles prepared in this comparative example is as follows Figure 8 As shown, the lithium cobalt oxide particles are hemispherical and have different particle sizes, rough surfaces and various shapes.

[0070] Comparative Example 3: The rest is the same as Example 1, except that:

[0071] The volume ratio of ethylene glycol methyl ether to monoethanolamine is 15:1.

[0072] The morphology of the lithium cobalt oxide particles prepared in this comparative example is as follows Fig. 9 As shown, the lithium cobalt oxide particles are of different sizes, and the particles are fused to form larger blocks.

[0073] Comparative Example 4: The rest is the same as Example 1, except that.

[0074] Diethanolamine was used in place of monoethanolamine.

[0075] The morphology of the lithium cobalt oxide particles prepared in this comparative example is as follows Fig.10 As shown, lithium cobalt oxide is an irregular sphere with obvious bumps on the surface.

[0076] Comparative Example 5: The rest is the same as Example 1, except that.

[0077] Triethanolamine was used instead of monoethanolamine.

[0078] The morphology of the lithium cobalt oxide particles prepared in this comparative example is as follows Fig.11 As shown, lithium cobalt oxide has an irregular morphology and a rough surface.

[0079] The lithium cobalt oxide particles prepared in Examples 1-6 and Comparative Examples 1-5 were respectively used as cathode materials to prepare button batteries. The preparation method of the button batteries is as follows:

[0080] (1) Lithium cobalt oxide particles, acetylene black and polyvinylidene fluoride (weight ratio of 80:10:10) were mixed in N-methylpyrrolidone, and the mixture was fully mixed to obtain a slurry with a viscosity of 6000-8000 mPa.s.

[0081] (2) The slurry was coated on aluminum foil and placed in vacuum ovens at 110°C, 130°C and 100°C respectively. The drying time at each temperature was 5 min. The electrode was dried and then punched and rolled to obtain the electrode.

[0082] (3) The button cell was assembled in an argon-filled glove box, using lithium metal foil as the counter electrode and polypropylene film (Celgard 2400) as the separator. The electrolyte was a mixture of ethyl carbonate (EC) and dimethyl carbonate (DMC) with a final concentration of 1 mol / L.

[0083] The button cells prepared with different lithium cobalt oxide particles were charged and discharged on the LAND battery test system at room temperature with a voltage window of 3.0-4.50V and 0.1C. The charging process included constant current charging and constant voltage charging: constant current charging was performed until the required voltage was reached, and constant voltage charging was performed until the current dropped to one tenth of the constant current value. The results are shown in Table 1 and Figure 12-13 As shown:

[0084] Table 1 The gram capacity of button batteries prepared with different lithium cobalt oxide particles

[0085] Group Gram capacity (mAh / g) Example 1 196 Example 2 193 Example 3 191 Example 4 192 Example 5 191 Example 6 190 Comparative Example 1 171 Comparative Example 2 160 Comparative Example 3 135 Comparative Example 4 143 Comparative Example 5 161

[0086] From the results in Table 1, it can be seen that the gram capacity of Examples 1-6 is significantly better than that of Comparative Examples 1-5, mainly due to:

[0087] The surface of the lithium cobalt oxide particles prepared in Example 1-6 is smooth and the particle size and morphology are uniform. When high-density compaction is performed in the preparation of the battery cell, the stress generated between the particles is small, which reduces the local strain and is beneficial to the Li + It shuttles back and forth between the positive and negative electrodes, thereby increasing the gram capacity to over 190mAh / g.

[0088] Comparative Example 1 has a rough surface that increases surface stress, resulting in local strain and hindering the Li + The shuttle of the body will affect the performance of the gram capacity.

[0089] Excessive monoethanolamine in Comparative Example 2 resulted in its + The complexation reaction is enhanced, Co + The electrons are obtained to form an outer circle of 18 electrons, which is a stable structure, and it is difficult to re-detach and participate in the synthesis reaction of lithium cobalt oxide particles. Therefore, there may be a large number of impurities in the synthesized lithium cobalt oxide particles, and the morphology is irregular spherical particles, which affects the performance of the battery cell, and the gram capacity is only 150mAh / g.

[0090] In Comparative Example 3, too little monoethanolamine makes it difficult to maintain the stable existence of ions in the solution. When the temperature begins to rise, the rapid movement of ions is difficult to control, thereby accelerating the formation of crystals and synthesizing irregular lithium cobalt oxide particles, resulting in a decrease in gram capacity.

[0091] Comparative Examples 4 and 5 show that diethanolamine and triethanolamine, which are similar in structure to monoethanolamine, cannot achieve the same effect as monoethanolamine.

Claims

1. A method for preparing lithium cobalt oxide, characterized in that: The steps include: (1) adding lithium salt, cobalt salt and organic acid to a mixture of ethylene glycol methyl ether and monoethanolamine to obtain a precursor solution; (2) Calcinate the precursor solution to obtain lithium cobalt oxide.

2. The method for preparing lithium cobalt oxide according to claim 1, characterized in that: In step (1), the volume ratio of ethylene glycol methyl ether to monoethanolamine in the mixed solution of ethylene glycol methyl ether and monoethanolamine is 5-15:

1.

3. The method for preparing lithium cobalt oxide according to claim 1, characterized in that: In step (1), the lithium salt includes at least one of lithium acetate, lithium phosphate, lithium carbonate, lithium chloride, lithium sulfate, and lithium nitrate; the cobalt salt includes at least one of cobalt nitrate, cobalt carbonate, cobalt sulfate, and cobalt chloride; and the organic acid includes at least one of citric acid, malic acid, acetic acid, formic acid, and oxalic acid.

4. The method for preparing lithium cobalt oxide according to claim 1, characterized in that: In step (1), the molar ratio of the lithium salt, the cobalt salt and the organic acid is 1-3:0.5-1.5:1-2.

5.

5. The method for preparing lithium cobalt oxide according to claim 1, characterized in that: In step (1), the mass ratio of the total weight of the lithium salt, the cobalt salt and the organic acid to the mixed solution of ethylene glycol methyl ether and monoethanolamine is 1-10:2-100.

6. The method for preparing lithium cobalt oxide according to claim 1, characterized in that: In step (2), the calcination method is: in an air environment, the temperature is raised to 750-850°C at a rate of 1-3°C / min, and the temperature is kept for 6-24 hours.

7. Use of the lithium cobalt oxide powder prepared according to the preparation method according to any one of claims 1 to 6 in preparing electrodes.

8. The use according to claim 7, characterized in that: The steps include: (1) adding the lithium cobalt oxide powder obtained by the preparation method according to any one of claims 1 to 6, a conductive agent and a binder into N-methylpyrrolidone and mixing them thoroughly to obtain a slurry; (2) The slurry is coated on a substrate, vacuum dried, and then rolled to obtain an electrode.

9. The use according to claim 8, characterized in that: The conductive agent is selected from at least one of acetylene black, graphite and carbon black; the binder is selected from at least one of polyvinylidene fluoride, polytetrafluoroethylene and sodium carboxymethyl cellulose; and the substrate is selected from at least one of aluminum foil, copper foil, carbon cloth and carbon paper.

10. A battery comprising the electrode according to claim 7.