Composition for preparing board, density board and preparation method of density board
By using alkali/acid that fast harden high temperature coagulation and hardening, geological polymer mineral gelling materials are stimulated as binders, and absorbing biomass formaldehyde through the exciter, the formaldehyde release problem of density plates is solved, and zero formaldehyde release and wood debris resources are achieved. The effective use of the environment improves the safety and resource utilization rate of environmentally friendly wooden density boards.
Patent Information
- Application Number
- CN202411158676.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-26
- Publication Date
- 2024-11-29
AI Technical Summary
During the production and use of LDL, the organic binders such as urea and formaldehyde resins will slowly release harmful volatile organic compounds such as formaldehyde, which will affect the health of production workers and consumers. In addition, the formaldehyde accumulated by biochemical reactions in natural wood materials leads to environmental pressure. Enlarge.
The alkali/acid-energic geological polymer mineral gelling materials are used as binders and absorbed and grown through the exciter The substance formaldehyde can realize the preparation of plant fiberboard with zero-release formaldehyde and the effective utilization of wood debris resources.
The preparation of environmentally friendly wooden density boards with zero release of formaldehyde has been achieved, which improves production safety and resource utilization, and reduces the ecological pressure on the environment.
Smart Images

Figure BDA0005005814590000071 
Figure BDA0005005814590000081
Abstract
Description
Technical Field
[0001] The invention belongs to the field of artificial boards, and in particular relates to a composition for preparing boards, a density board and a preparation method thereof. Background Art
[0002] Density board is a board made by applying urea-formaldehyde resin and other synthetic resins to fiber raw materials under heating and pressure conditions. Density board has good physical and mechanical properties and processing properties, and can be made into boards of different thicknesses. Therefore, it is widely used in furniture manufacturing, construction, interior decoration, etc. However, during the production and use process, due to the use of organic binders such as urea-formaldehyde resin and the accumulation of formaldehyde in natural wood materials due to biochemical reactions, density boards will slowly release a certain amount of formaldehyde and other harmful volatile organic compounds, which seriously affect the health of production workers and consumers. Therefore, seeking a new type of environmentally friendly wood density board without formaldehyde release is of great significance to alleviate ecological pressure and improve people's living environment. Summary of the invention
[0003] In view of the above problems, the present invention innovatively proposes to use alkali / acid-activated geopolymer mineral cementitious materials as binders, which have rapid high-temperature coagulation and hardening, high early and late strength, good bonding properties, small shrinkage, high temperature resistance and good freeze-thaw resistance, so as to achieve zero formaldehyde emission of the binder with mineral cementitious materials, and use stimulants to absorb biomass formaldehyde, so as to strive to achieve the preparation of formaldehyde-free plant fiberboard and the effective utilization of wood debris resources.
[0004] In a first aspect, the present invention provides a composition for preparing a board material, the composition comprising fiber powder, aluminosilicate mineral powder, an activator and an organic emulsion, wherein the activator is selected from an alkaline activator and an acidic activator.
[0005] According to some embodiments of the above composition, the aluminosilicate mineral powder minerals are selected from calcined kaolin and low-calcium fly ash, preferably calcined kaolin calcined at 600-750°C.
[0006] According to some embodiments of the above composition, the aluminosilicate mineral powder is natural kaolin and calcined kaolin, and based on the mass of dry powder, the silicon oxide content is 45-55% by weight, the aluminum oxide content is 35-45% by weight, and the total content of silicon oxide and aluminum oxide should be greater than 85% by weight.
[0007] According to some embodiments of the above composition, the aluminosilicate mineral powder is fly ash, and based on the dry powder mass, the silicon oxide content is 45-60% by weight, the aluminum oxide content is 20-35% by weight, and the calcium oxide content is less than 10% by weight.
[0008] According to some embodiments of the above composition, the fiber powder is selected from natural fiber powder, preferably selected from wood fiber powder and plant fiber powder, preferably wood fiber powder.
[0009] According to some embodiments of the above composition, the fiber powder is derived from one or more of poplar, pine, fir, birch, elm, ash, wheat straw, rice straw and bagasse.
[0010] According to some embodiments of the above composition, the fiber powder has a length in the range of 5-15 mm and a particle size in the range of 1-4 mm.
[0011] According to some embodiments of the above composition, the alkaline activator is selected from alkali metal hydroxide solution and soluble silicate solution, and is used alone or in combination of multiple activators. Preferably, the activator is an alkali metal hydroxide-soluble silicate mixed solution.
[0012] According to some embodiments of the above composition, the activator can be an alkali metal hydroxide solution, a soluble silicate solution, used alone or in combination of multiple activators, preferably an alkali metal hydroxide-soluble silicate mixed solution is the activator.
[0013] According to some embodiments, in the composite solution of alkali metal hydroxide-soluble silicate, (calculated based on the total amount of activator),
[0014] Alkali metal hydroxide proportion: 5-20% by weight;
[0015] Silicate solution proportion: 25-95% by weight;
[0016] Additional water content: 20-5% by weight;
[0017] Alkali metal hydroxide solution concentration alone: (calculated based on the total amount of activator) 5% to 50%;
[0018] Concentration of single soluble silicate solution: (calculated based on the total amount of activator) 10% to 40%;
[0019] The soluble silicate modulus (molar ratio of silicon oxide to alkali metal oxide in silicate) = 1.0 to 4.0.
[0020] According to some embodiments of the above composition, the content of the alkaline activator is 100-200 weight % based on the total weight of the aluminosilicate mineral powder.
[0021] According to some embodiments of the above composition, the acidic activator is selected from phosphoric acid, hydrogen phosphate and dihydrogen phosphate aqueous solution, and phosphoric acid is preferably used as the activator.
[0022] According to some embodiments of the above composition, the concentration of the acidic activator solution is between 10 and 80 weight %.
[0023] According to some embodiments of the above composition, the mass ratio of the acidic activator solution to the aluminosilicate mineral powder is between 0.8 and 1.2.
[0024] According to some embodiments of the above composition, based on the total weight of the fiber powder and the aluminosilicate mineral powder, the content of the aluminosilicate mineral powder is 15-60% by weight, the content of the fiber powder is 40-85% by weight, the content of the activator is 100-200% by weight, and the content of the organic emulsion is 0.5-10% by weight.
[0025] According to some embodiments of the above composition, when the activator is an acidic activator, the content of the activator is 120-200% by weight, and when the activator is an alkaline activator, the content of the activator is 100-200% by weight.
[0026] According to some embodiments of the above composition, the weight ratio of the aluminosilicate mineral powder to the fiber powder is 1:5-1:1.5, preferably 2:1-1:1.5, and most preferably 1.5:1-1:1.
[0027] According to some embodiments of the above composition, the composition further comprises a water-proofing agent.
[0028] According to some embodiments of the above composition, the content of the waterproofing agent is 0.5-10% by weight, based on the total weight of the fiber powder and the aluminosilicate mineral powder.
[0029] According to some embodiments of the above composition, the organic emulsion is selected from acrylate emulsion and its derivatives, styrene-acrylate emulsion and its derivatives, butadiene-styrene copolymer and its derivatives, ethylene-vinyl acetate copolymer and its derivatives, preferably styrene-acrylate emulsion and its derivatives.
[0030] According to some embodiments of the above composition, the amount of the organic emulsion added is 0.5-10% by weight based on the total weight of the fiber powder and the aluminosilicate mineral powder.
[0031] According to some embodiments of the above composition, the waterproofing agent is selected from organosilane waterproofing agents and long-chain fatty acid salt waterproofing agents, and preferably, its dosage is 0.5-10 weight % based on the total weight of the fiber powder and the aluminosilicate mineral powder.
[0032] The second aspect of the present invention provides use of the above composition for preparing a board, preferably a density board.
[0033] The third aspect of the present invention provides a density board, which includes a geopolymer layer formed by silicate mineral powder and an activator and a fiber mesh layer. Preferably, the fiber mesh is selected from polypropylene fiber mesh, polyethylene fiber mesh, polyvinyl alcohol fiber mesh and glass fiber mesh, and the hole diameter of the fiber mesh is preferably 2-5 mm.
[0034] The aluminosilicate mineral powder minerals are calcined kaolin and low-calcium fly ash, preferably calcined kaolin calcined at 600-750°C.
[0035] According to some embodiments of the above-mentioned density board, the aluminosilicate mineral powder minerals are natural kaolin and calcined kaolin, and based on the mass of dry powder, the silicon oxide content is 45-55% by weight, the aluminum oxide content is 35-45% by weight, and the total content of silicon oxide and aluminum oxide should be greater than 85% by weight.
[0036] According to some embodiments of the density board, the aluminosilicate mineral powder is fly ash, and based on the dry powder mass, the silicon oxide content is 45-60% by weight, the aluminum oxide content is 20-35% by weight, and the calcium oxide content is less than 10% by weight.
[0037] The fourth aspect of the present invention provides a method for preparing a board, preferably a density board, comprising pressing the composition described in the first aspect of the present invention with a fiber grid, preferably comprising the following steps:
[0038] (1) mixing fiber powder and aluminosilicate mineral powder to obtain a first mixture,
[0039] (2) mixing the first mixture with an activator, an organic emulsion and an optional water-proofing agent to obtain a second mixture;
[0040] (3) placing the second mixture and the fiber grid in a mold for compression molding. Preferably, the reinforced mold after compression molding is subjected to pressurized steam curing.
[0041] According to some embodiments of the above method, the compression molding includes: after the second mixture and the fiber grid are laid, the mold is covered, and when the pressure is loaded to 1-5MPa at a rate of 0.05-0.5MPa / s, the pressurization is stopped and maintained for 2-10 minutes.
[0042] According to some embodiments of the above method, the pressure curing comprises curing the reinforced mold in an environment of 40-80° C. for 1-10 hours, and demolding after cooling.
[0043] According to some embodiments of the above method, the fiber mesh can be a polypropylene fiber mesh, a polyethylene fiber mesh, a polyvinyl alcohol fiber mesh, a glass fiber mesh, etc. The hole diameter of the fiber mesh is selected to be 2-5 mm, and a glass fiber mesh is preferred.
[0044] The present invention adopts alkali / acid-activated geopolymer mineral cementitious material as a binder, which has rapid high-temperature coagulation and hardening, high early and late strength, good bonding performance, small shrinkage, high temperature resistance and good freeze-thaw resistance, and achieves zero formaldehyde emission of the binder with the mineral cementitious material, and adopts an activator to absorb biomass formaldehyde, thereby realizing the preparation of formaldehyde-free plant fiberboard and the effective utilization of wood debris resources. DETAILED DESCRIPTION
[0045] The present invention is described in detail below with reference to the embodiments, but the present invention is not limited to the following embodiments.
[0046] [Example 1]
[0047] Accurately weigh each substance, taking the total weight of the dry powder material as the benchmark, the weight of the pine wood fiber chips is 70 weight%, the weight of the calcined kaolin powder is 30 weight%, the dosage of the styrene-acrylate emulsion is 0.5 weight%, the dosage of the silane waterproofing agent is 0.5 weight%, and the total weight of the calcined kaolin powder is used as the benchmark, and the dosage of the alkali metal hydroxide-soluble silicate activator solution is 100 weight%.
[0048] Among them, based on the total weight of the activator, the content of sodium hydroxide solid particles is 9.3 weight %, the content of 38% industrial sodium silicate solution (the ratio of silicon oxide to aluminum oxide is 3.4) is 82.5 weight %, and the content of added water is 8.2 weight %.
[0049] (A) Premixing of wood fiber debris and aluminosilicate mineral powder:
[0050] According to the weight ratio of each component, each component is accurately weighed, and the pine wood fiber chips and calcined kaolin powder are placed in a mechanical mixer at room temperature for 0.5 h to ensure that the powder is evenly distributed.
[0051] (B) Mixing:
[0052] Accurately weigh the activator solution, styrene-acrylate emulsion and silane waterproofing agent, place the above components in a container and mix them evenly. Then, place the premixed powder obtained in step (A) in a planetary mixer and add the mixed solution, and stir thoroughly for 5 minutes until the mixture is evenly mixed.
[0053] (C) Moulding:
[0054] Before molding, a mold release agent is sprayed in the mold of the cold press, preferably, the mold release agent is methyl silicone oil. Subsequently, the uniformly mixed semi-dry material obtained in step (B) is first evenly spread to half the depth of the cold press mold, and the remaining material is filled into the mold after the fiber grid is laid.
[0055] (D) Pressing molding:
[0056] After the material and fiber mesh are laid, the mold is covered and loaded at a rate of 0.05MPa / s to 1MPa, then the pressurization is stopped. After maintaining for 5 minutes, the mold and the top cover are reinforced with screws to maintain the pressure.
[0057] (E) Pressure curing:
[0058] The reinforced mold obtained in step (D) is placed in an environment of 80° C. for steam curing for 3 hours, demoulded after cooling, and cut as needed to obtain the required geopolymer bonded density board.
[0059] [Example 2]
[0060] Accurately weigh each substance, with the total weight of the dry powder material as the benchmark, the weight of the pine wood fiber chips is 70 weight%, the weight of the calcined kaolin powder is 30 weight%, the dosage of the styrene-acrylate emulsion is 0.5 weight%, the dosage of the silane waterproofing agent is 0.5 weight%, and the total weight of the calcined kaolin powder is used as the benchmark, and the dosage of the phosphoric acid activator solution is 80 weight%.
[0061] Wherein, based on the total weight of the phosphoric acid activator solution, the content of phosphoric acid is 70 weight %.
[0062] (A) Premixing of wood fiber debris and aluminosilicate mineral powder:
[0063] According to the weight ratio of each component, each component is accurately weighed, and the pine wood fiber chips and calcined kaolin powder are placed in a mechanical mixer at room temperature for 0.5 h to ensure that the powder is evenly distributed.
[0064] (B) Mixing:
[0065] Accurately weigh the phosphoric acid activator solution, styrene-acrylate emulsion and silane waterproofing agent, place the above components in a container and mix them evenly. Then, place the premixed powder obtained in step (A) in a planetary mixer and add the mixed solution, and stir thoroughly for 5 minutes until the mixture is evenly mixed.
[0066] (C) Moulding:
[0067] Before molding, a mold release agent is sprayed in the mold of the cold press, preferably, the mold release agent is methyl silicone oil. Subsequently, the uniformly mixed semi-dry material obtained in step (B) is first evenly spread to half the depth of the cold press mold, and the remaining material is filled into the mold after the fiber grid is laid.
[0068] (D) Pressing molding:
[0069] After the material and fiber mesh are laid, the mold is covered and loaded at a rate of 0.05MPa / s to 1MPa, then the pressurization is stopped. After maintaining for 5 minutes, the mold and the top cover are reinforced with screws to maintain the pressure.
[0070] (E) Pressure curing:
[0071] The reinforced mold obtained in step (D) is placed in an environment of 80° C. for steam curing for 6 hours, demoulded after cooling, and cut as needed to obtain the required geopolymer bonded density board.
[0072] [Example 3-5]
[0073] The method of Example 1 is followed, except that the parameters of the wood fiber chips and the aluminosilicate mineral powder are shown in Table 1.
[0074] [Examples 6-8]
[0075] The method of Example 2 is followed, except that the parameters of the wood fiber chips and the aluminosilicate mineral powder are shown in Table 1.
[0076] [Examples 9-11]
[0077] The method of Example 1 is followed, except that the parameters of the organic emulsion and the waterproofing agent are shown in Table 1.
[0078] [Examples 12-14]
[0079] The method of Example 2 is followed, except that the parameters of the organic emulsion and the waterproofing agent are shown in Table 1.
[0080] [Examples 15-16]
[0081] The method of Example 1 is followed, except that the parameters of the alkali metal hydroxide-soluble silicate solution are shown in Table 1.
[0082] [Examples 17-18]
[0083] The method of Example 2 is followed, except that the parameters of the phosphoric acid activator solution are shown in Table 1.
[0084] [Comparative Example 1]
[0085] The method of Example 1 is followed, except that no organic emulsion and waterproofing agent are added. Parameters are shown in Table 1.
[0086] [Comparative Example 2]
[0087] The method of Example 2 is followed, except that no organic emulsion and waterproofing agent are added. Parameters are shown in Table 1.
[0088] [Examples 19-21]
[0089] The method of Example 1 is followed, except that the parameters for changing the type of wood fiber chips are shown in Table 1.
[0090] [Examples 22-24]
[0091] The method of Example 2 is followed, except that the parameters of the wood fiber debris type are changed as shown in Table 1.
[0092]
Test example
[0093] According to the national standard GB / T 17657-2013 "Test methods for physical and chemical properties of wood-based panels and veneer wood-based panels", the plant fiber boards prepared in Examples 1-13 and Comparative Examples 1-5 were tested for static bending strength, water absorption expansion rate, dimensional stability, moisture content, formaldehyde emission, internal bonding strength, and cigarette burn grade (surface cigarette burn resistance). The results are shown in Table 2.
[0094] Table 1
[0095]
[0096] The weight percentages of wood fiber chips, aluminosilicate powder, organic emulsion and waterproofing agent in Table 1 are based on the total weight of dry powder materials; the weight percentage of alkali metal hydroxide-soluble silicate activator is based on the total weight of aluminosilicate powder.
[0097] Table 2
[0098]
[0099] Although the present invention has been described above with reference to some embodiments, various modifications may be made without departing from the scope of the present invention. The present invention is not limited to the specific embodiments disclosed herein, but to all technical solutions falling within the scope of the claims.
Claims
1. A composition for preparing a board material, comprising fiber powder, aluminosilicate mineral powder, an activator and an organic emulsion, wherein the activator is selected from an alkaline activator and an acidic activator.
2. The composition according to claim 1, It is characterized in that The fiber powder is selected from natural fiber powder, preferably selected from wood fiber powder and plant fiber powder, preferably wood fiber powder; preferably, the fiber powder is derived from one or more of poplar, pine, fir, birch, elm, ash, wheat straw, rice straw and bagasse; and / or The length of the fiber powder is in the range of 5-15 mm, and the particle size is in the range of 1-4 mm.
3. The composition according to claim 1 or 2, It is characterized in that Alkali metal hydroxide solution, soluble silicate solution, used alone or in combination with multiple activators, preferably alkali metal hydroxide-soluble silicate mixed solution as the activator, and / or Based on the total weight of the aluminosilicate mineral powder, the content of the alkaline silicate activator is 100-200 weight %; and / or The acidic activator is selected from phosphoric acid, hydrogen phosphate and dihydrogen phosphate aqueous solution, preferably phosphoric acid is the activator, and / or The concentration of the acidic activator solution is between 10 and 80% by weight, and / or The mass ratio of the acidic activator solution to the aluminosilicate mineral powder is between 0.8 and 1.
2.
4. A composition according to any one of claims 1 to 3, It is characterized in that Based on the total weight of the fiber powder and the aluminosilicate mineral powder, the content of the aluminosilicate mineral powder is 15-60% by weight, the content of the fiber powder is 40-85% by weight, the content of the activator is 100-200% by weight, and the content of the organic emulsion is 0.5-10% by weight; Preferably, when the activator is an acidic activator, the content of the activator is 120-200% by weight, and when the activator is an alkaline activator, the content of the activator is 100-200% by weight; Preferably, the weight ratio of the aluminosilicate mineral powder to the fiber powder is 1:5-1:1.5, preferably 2:1-1:1.5, and most preferably 1.5:1-1:
1.
5. A composition according to any one of claims 1 to 4, It is characterized in that Also includes water repellent, Preferably, the content of the waterproofing agent is 0.5-10% by weight based on the total weight of the fiber powder and the aluminosilicate mineral powder.
6. A composition according to any one of claims 1 to 5, It is characterized in that The organic emulsion is selected from acrylate emulsion and its derivatives, styrene-acrylate emulsion and its derivatives, butadiene-styrene copolymer and its derivatives, ethylene-vinyl acetate copolymer and its derivatives, preferably styrene-acrylate emulsion and its derivatives, preferably, its addition amount is 0.5-10 weight% based on the total weight of fiber powder and aluminosilicate mineral powder; and / or The waterproofing agent is selected from organic silane waterproofing agents and long-chain fatty acid salt waterproofing agents. Preferably, the amount thereof is 0.5-10% by weight based on the total weight of the fiber powder and the aluminosilicate mineral powder.
7. Use of the composition according to any one of claims 1 to 6 for preparing a board, preferably a density board.
8. A density board comprising a geopolymer layer formed by aluminosilicate mineral powder and an activator and a fiber mesh layer, preferably, the fiber mesh is selected from polypropylene fiber mesh, polyethylene fiber mesh, polyvinyl alcohol fiber mesh and glass fiber mesh, and the hole diameter of the fiber mesh is preferably 2-5 mm.
9. The method for preparing a density board according to claim 8, comprising pressing and molding the composition according to any one of claims 1 to 6 with a fiber grid, preferably The following steps are involved: (1) mixing fiber powder and aluminosilicate mineral powder to obtain a first mixture, (2) mixing the first mixture with an activator, an organic emulsion and an optional water-proofing agent to obtain a second mixture; (3) placing the second mixture and the fiber grid in a mold for compression molding. Preferably, the reinforced mold after compression molding is subjected to pressurized steam curing.
10. The method according to claim 9, It is characterized in that The compression molding includes, after the second mixture and the fiber grid are laid, covering the mold, and when the pressure is loaded to 1-5MPa at a rate of 0.05-0.5MPa / s, stopping the pressurization and maintaining it for 2-10 minutes; the pressurized steam curing includes steam curing the reinforced mold in an environment of 40-80°C for 1-10 hours, and demolding after cooling.
Citation Information
Patent Citations
Method for preparing geopolymer and organic macromolecule composite gelled material
CN101544485A
Organic additive, and preparation method and applications thereof
CN106396460A
Geopolymer-based rice straw fiber board and preparation method thereof
CN107555870A
Plant fiber artificial board and preparation method and application thereof
CN110900778A
A composition for preparing the hybrid composite board using wood fiber and geopolymer and the hybrid composite board
KR1020110057832A