High-refractive-index thioether type episulfide compound as well as preparation method and application thereof
Through in-situ polymerization of sulfide type cyclic sulfur compounds with isothiocyanate or isocyanate, the problems of low purity and complex process of existing high-refractive index thiol compounds are solved, and polyurethane optical with high refractive index and low color are prepared Material, suitable for a variety of optical substrates, meeting the needs of high-end optical components.
Patent Information
- Application Number
- CN202411227033.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-03
AI Technical Summary
In the synthesis process of existing high-refractive index thiol compounds, there are problems such as low purity, many by-products, complex process and high cost, which is difficult to meet the needs of high-end optical components.
The structure of a sulfide-type cyclic sulfur compound is adopted for in-situ polymerization with isothiocyanate or isocyanate. Through specific synthesis steps and catalyst control, a high refractive index polyurethane optical material is prepared with high refractive index and light transmittance. , suitable for a variety of optical substrates.
The preparation of polyurethane optical materials with high refractive index and light transmittance has high purity, low chromaticity and good polymerization performance. It is suitable for high-end optical components, reducing production costs and process complexity.
Smart Images

Figure CN119039269A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of synthesis and preparation of polyurethane optical materials, and specifically relates to a high-refractive-index thioether-type episulfide compound and a preparation method and application thereof. Background Art
[0002] Lightweighting of optical systems means reducing the curvature, thickness and weight of optical equipment as much as possible while ensuring optical performance and functions, so as to miniaturize, refine and integrate optical devices. Improving the refractive index is an important means to achieve lightweighting. Western developed countries are at the world's leading level due to their early research. For example, Japan's Mitsui Chemicals uses trivalent thiol with mercapto (-SH) instead of hydroxyl to react with isocyanate to prepare high-refractive-index polyurethane resin (product number MR), with a refractive index ranging from 1.67-1.76, and its products have long occupied the global market; U.S. Patent [US2011046285] discloses the use of epoxy compounds and thiocyanates to react to prepare high-refractive, high-epoxy compound monomers.
[0003] The refractive index is inversely proportional to the molecular volume and proportional to the molar refractive index, which is proportional to the polarizability of the medium. To increase the refractive index of the resin, the main method is to introduce groups with higher molar refractive index and smaller molecular volume into the molecular structure of the polymer. High-refractive polyurethane has overcome the opacity of traditional polyurethane and has the characteristics of high light transmittance, high strength and good impact resistance. It is widely used in high-end optical fields such as optical lenses, instrument prisms, light filtering protection, LED lighting, smart cars and window materials. In recent years, there have been many reports on the introduction of sulfur atoms through molecular design to increase the refractive index of thiol monomers. Due to the existence of d orbitals in the outer layer of sulfur atoms, the two pairs of electrons in the outermost layer are easily polarized, which makes the sulfur atoms have both low molecular dispersion and high molecular refractive index.
[0004] The following are some examples of methods for synthesizing high sulfur compound monomers.
[0005] (1) Alkyl halide reacts with sodium hydrosulfide in an alcohol solution to produce mercaptan, as shown in formula (1). This method has a high reaction temperature, sodium hydrosulfide is unstable at high temperatures and easily decomposes into Na2S, and it is also easy to generate by-products, making the production process difficult to control.
[0006]
[0007] (2) Alkyl halides react with thioacids under certain conditions to form thiol esters. - or H + Under certain conditions, it is hydrolyzed into thiol, as shown in formula (2). However, this method has a low yield and high cost, which is not conducive to industrial-scale production.
[0008]
[0009] (3) The mercaptoethanol reacts with trichloropropane, refluxes and reacts with a KOH solution containing ME, separates the liquids and refluxes under reduced pressure to obtain 1,2,3-mercaptoethylthiopropane. However, mercaptoethanol is easily oxidized under high temperature and alkaline conditions to generate complex by-products, which causes the mercaptan to turn yellow, affecting the use of the product.
[0010] (4) Using sulfur monochloride and mercaptoethanol as raw materials and petroleum ether as solvent, diethyl tetrasulfide is generated through condensation, and isothiourea salt is obtained, which is then hydrolyzed to obtain tetrathio-based polythiol. This method is complex and has high production costs. In addition, the use of a large amount of toxic solvents is not conducive to environmental protection.
[0011] Among the thiol compounds synthesized by the above chemical reactions, some use cyclosulfide compounds with a higher sulfur content to achieve the preparation of optical materials with a higher refractive index, and some have a maximum refractive index of even more than 1.85, which has achieved important breakthroughs. However, there is still a problem of low purity of the cyclosulfide monomers produced. The synthesis process is often accompanied by other side reactions, resulting in low product purity and inability to be used as optical materials. It is difficult to separate them from complex mixed systems by traditional extraction, distillation and other methods alone, or the synthetic monomers are not stable enough, and agglomeration or self-polymerization occurs during storage, affecting their use in the field of high-end optical components. Some have problems such as harsh synthesis process conditions, and large-scale production is difficult. Therefore, advanced synthesis methods and technologies will increasingly show their importance in the development and application of new cyclosulfide compounds. Summary of the invention
[0012] In view of the above problems in the prior art, the present invention provides a thioether-type episulfide compound, whose refractive index reaches 1.66-1.76. The compound or a mixture thereof is in-situ polymerized with isothiocyanate or isocyanate to prepare a high refractive index polyurethane optical material, which has the advantages of high refractive index and light transmittance, low chroma, and strong comprehensive performance, and can be used for a variety of different optical substrates, providing a wider range of material selection for the application of high-end optical components.
[0013] To achieve the above object, the present invention provides the following technical solutions: A high refractive index thioether type episulfide compound, the structure of the compound is shown in Formula I, Formula II or Formula III:
[0014] (I) Wherein R and R1 are the same or different and are each H, CH3 or C6H5;
[0015] (II)
[0016] (III) Wherein R is H or CH3.
[0017] On the other hand, the present invention provides a method for preparing the high refractive index thioether-type episulfide compound I as described above, the method comprising the following steps: ⑴ Add 1,3-diphenylacetone and anhydrous ethanol in a weight ratio of (1-3): (3-7) into a reaction vessel, stir evenly, and introduce hydrogen sulfide and hydrogen chloride dry gas for 3-7 hours. The reaction temperature is controlled at 0-6°C. After 10-12 hours, the precipitate is vacuum dried to obtain a thiol intermediate; (2) The thiol intermediate, benzaldehyde and diethyl ether are fully mixed in a weight ratio of (1-2): (1-2): (100-150), and a catalyst in an amount of 1 / 8-1 / 12 of the weight of the thiol intermediate is added thereto, and the reaction is stopped after being fully stirred at room temperature for 7-10 hours. A saturated sodium chloride solution is then added, and after stirring and mixing to separate layers, the upper diethyl ether layer is taken out, dried, and decolorized with a concave clay adsorbent until it becomes colorless and transparent, and the diethyl ether solvent is removed by distillation to obtain a viscous thioether-type tricyclic sulfide compound I.
[0018] In the method for preparing the high refractive index thioether-type episulfide compound I as described above, preferably, the catalyst is one of hydrochloric acid, sulfuric acid, toluenesulfonic acid and p-toluenesulfonic acid.
[0019] In another aspect, the present invention provides a method for preparing the high refractive index thioether-type episulfide compound II as described above, the method comprising the following steps: ⑴ Add 1,3-diphenylacetone and anhydrous ethanol in a weight ratio of (1-3): (3-7) into a reaction vessel, stir evenly, and introduce hydrogen sulfide and hydrogen chloride dry gas for 3-7 hours. The reaction temperature is controlled at 0-6°C. After 10-12 hours, the precipitate is vacuum dried to obtain a thiol intermediate; ⑵ Add anhydrous ethanol and thiol intermediate to the reaction vessel. After they are fully dissolved, add ferric chloride and water. The weight ratio of thiol intermediate, ethanol, ferric chloride and water is (1-3): (2-5): (2-4): (2-3). Stir and react at 0-10°C for 4-6 hours. A white powdery substance precipitates. Filter and obtain a crude product. Recrystallize with n-hexane and dry in vacuo to obtain thioether-type tetracyclic sulfur compound II.
[0020] In another aspect, the present invention provides a method for preparing the high refractive index thioether-type episulfide compound III as described above, the method comprising the following steps: adding sodium pentathiocarbonate to methanol, heating to 25-45° C. after complete dissolution, dripping dibromomethane methanol solution within 1.5-2.5 hours, slowly stirring and reacting for about 30-35 hours; the weight ratio of sodium pentathiocarbonate, methanol and dibromomethane methanol solution is (1-3): (2-5): (3-7), and the concentration of dibromomethane methanol solution is 6-12wt%; adding distilled water to the reaction system, extracting with chloroform, combining the extracts, and removing chloroform by atmospheric distillation to obtain a colloidal thioether-type episulfide compound III.
[0021] Chloroform is selected as the extraction solvent in the extraction process mainly because the solvent has a large density and a low boiling point. The sodium bromide precipitate is dissolved and then removed with the water. The organic phase can quickly evaporate the solvent at normal pressure of 55-60°C, avoiding the generation of complex by-products of the episulfide monomer under high temperature conditions, which results in a darker color of the monomer and affects its use as an optical material.
[0022] In another aspect, the present invention provides the use of the high refractive index thioether type episulfide compound as described above as a polyurethane optical material, wherein the polyurethane optical material is polymerized by the high refractive index thioether type episulfide compound and an isothiocyanate compound and / or an isocyanate compound.
[0023] In the application as described above, preferably, the mass ratio of the high refractive index thioether type episulfide compound to the isothiocyanate compound, the isocyanate compound or a mixture thereof is (30-70):(10-50).
[0024] The sodium pentathiocarbonate of the present invention can be purchased through commercial channels, or can be prepared by the following method: dissolving sodium sulfide in anhydrous ethanol, adding carbon disulfide thereto, controlling the reaction under stirring at room temperature, adding sulfur under stirring, heating with microwaves at a temperature of 40-45° C., reacting for 20-60 minutes, cooling naturally to room temperature, adding n-pentane solution, and precipitating sodium pentathiocarbonate. Selecting low-density n-pentane during the reaction facilitates the precipitation of crystal precipitates.
[0025] The beneficial effects of the present invention are: (1) The raw materials required in the reaction process of the method of the present invention are abundant in domestic sources and are easy to purchase. The synthesis process is simple, the reaction conditions are mild and controllable, and there is no special customization requirement for the equipment required for production. Conventional equipment can now meet the requirements of the synthesis process, which reduces the cost of application to a certain extent.
[0026] ⑵ The prepared thioether episulfide compounds have high purity, light color, good homopolymerization and copolymerization properties. The highly cross-linked network formed during the polymerization process limits the crystallization of the groups, ensuring the high transparency of the polyurethane material.
[0027] (3) The polyurethane optical material polymerized from the thioether-type episulfide compound has the advantages of high transmittance, high refractive index and low chromaticity. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The FT-IR infrared spectrum of the tricyclic sulfide compound (i) prepared in a specific embodiment.
[0029] Figure 2 The HNMR nuclear magnetic resonance hydrogen spectrum of the tricyclic sulfide compound (i) prepared in a specific embodiment.
[0030] Figure 3 The FT-IR infrared spectrum of the tetracyclic sulfur compound (ii) prepared in a specific embodiment.
[0031] Figure 4 The FT-IR infrared spectrum of the pentacyclic sulfur compound (iii) prepared in a specific embodiment.
[0032] Figure 5 FIG. 4 is a refractive index curve of a thioether-type episulfide compound prepared in a specific embodiment. DETAILED DESCRIPTION
[0033] The present invention is further described below by means of specific examples, but this is not intended to limit the protection scope of the present invention.
[0034] The thioether-type episulfide compounds in the following examples are prepared by the following method: 1. Preparation of tricyclic sulfide compound (i): The specific reaction formula is as follows:
[0035] R, R1 is phenyl 900 g of 1,3-diphenylacetone and 1680 g of anhydrous ethanol were added to a reaction vessel, and after stirring evenly, hydrogen sulfide and hydrogen chloride dry gas were introduced for 6 h. The reaction temperature was controlled at 2°C. After 10 h, the precipitate was vacuum dried to obtain a thiol intermediate. 240 g of the thiol intermediate and 150 g of benzaldehyde were added to 25000 g of ether solvent, and then 24 g of p-toluenesulfonic acid was added thereto. After stirring at room temperature for 9 h, a saturated sodium chloride solution was added thereto. After stirring and layering, the upper light yellow ether layer was taken out, dried, and decolorized with a 150-mesh attapulgite adsorbent until transparent. The ether solvent was evaporated to obtain 149 g of tricyclic sulfide compound (i), with a yield of 61.3%.
[0036] Infrared spectra such as Figure 1 As shown, FT-IR (cm -1) analysis: 3060~3031 are CH stretching vibrations of benzene ring; 2902 are saturated CH stretching vibrations; 1601~1492 are C=C skeleton stretching vibrations of benzene ring; 1489 are CH2 shear vibrations; 745~697 are out-of-plane deformation vibrations of multiple adjacent H atoms =CH on the benzene ring and ring skeleton deformation vibrations; 579 are CS stretching vibrations.
[0037] HNMR nuclear magnetic resonance spectrum Figure 2 As shown, 1 H NMR (δ) analysis: 7.32 (m, 20H, Ar-H), 2.72 (s, 4H, CH2), δ = 7.24 ~ 7.34ppm, where δ = 7.32ppm means there are 20 hydrogen atoms (Ar-H), which are on the benzene ring and show multiple peaks (m); δ = 4.57ppm corresponds to a hydrogen connected to the sulfur heterocyclic ring in the tricyclic sulfur compound molecule, which shows a single peak because there are no hydrogen atoms on the adjacent carbon; δ = 2.72ppm shows a single peak (S) for the hydrogen on the saturated carbon atom, which belongs to the hydrogen on the methylene group (CH2), and the number is 4.
[0038] 2. Preparation of tetracyclic sulfur compounds (ii): The specific reaction formula is as follows:
[0039] (ii) 360 g of the thiol intermediate prepared in the above step was added to 1080 g of ethanol, and after dissolving, 820 g of ferric chloride and 650 g of water were added and stirred repeatedly. The temperature was controlled at 5° C. and the reaction was carried out for 4.5 h. The collected precipitate was recrystallized with n-hexane and dried in vacuo to obtain 186 g of tetracyclic sulfur compound (ii) with a yield of 51.5%.
[0040] Infrared spectra such as Figure 3 As shown, FT-IR (cm -1 ) analysis: 3055-3026 is the CH stretching vibration of the benzene ring; 2909 is the saturated CH stretching vibration; 1603-1556 is the C=C skeleton stretching vibration of the benzene ring; 1490 is the C=C stretching vibration of the benzene ring; 1450 is the CH2 shear vibration; 749-706 is the out-of-plane deformation vibration of the 5 adjacent H atoms =CH on the benzene ring and the ring skeleton deformation vibration; 587 is the CS stretching vibration; 508 is the SS stretching vibration.
[0041] 1 HNMR (δ): 7.37(m, 20H, Ar-H), 2.6(s, 8H, CH2).
[0042] 3. Preparation of pentacyclic sulfur compound (iii): The specific reaction process is as follows:
[0043] 2200 g of sodium sulfide was dissolved in 11000 g of anhydrous ethanol, and 2400 g of carbon disulfide was added. The mixture was stirred and reacted at room temperature. 160 g of sulfur was added with stirring, and the mixture was microwaved at 45° C. for 50 min. The mixture was naturally cooled to room temperature, and n-pentane solvent was added to precipitate sodium pentathiocarbonate. 1050 g of sodium pentathiocarbonate was added to 2400 g of methanol. After dissolution, the mixture was heated to 35° C., and 5200 g of 8% dibromomethane methanol solution was added dropwise within 2 h. The mixture was stirred and reacted for 31 h. Distilled water was added thereto, and the mixture was extracted with chloroform. The extracts were combined, dried over anhydrous sodium sulfate, and chloroform was removed by atmospheric distillation to obtain 318 g of pentacyclic sulfur compound (iii) with a yield of 45.4%.
[0044] Infrared spectra such as Figure 4 As shown, FT-IR (cm -1 ) analysis: 2955~2887 is the CH stretching vibration peak, 1380~1183 is the CH2 non-planar swing absorption peak on the ring; 809~596 is the CS stretching vibration strong absorption peak; 460 is the SS weak vibration absorption peak.
[0045] 1 HNMR (δ) analysis: 4.30 (s, 4H, 2CH2), the compound has a single peak at δ = 4.30 ppm, indicating that the two CH2 are in the same chemical environment, indicating that the compound has a symmetrical structure.
[0046] Example 1: Preparation of polyurethane optical material containing tricyclic sulfide compound monomer (i) ⑴ After heating 20 g of an isothiocyanate compound (Hunan Yunbang Biotechnology Co., Ltd., product number: YB06161, the same in the following embodiments) to 85° C., 15 g of xylene diisocyanate was added with stirring, and then 0.6 g of triethyldiamine was added, and the mixture was obtained after stirring evenly.
[0047] (2) 65 g of the tricyclic sulfide compound (i) prepared above was added to the mixture prepared in step (1), 1.6 g of dibutyltin dilaurate was added to the reaction product, and the mixture was heated to 45°C and stirred for prepolymerization for 35 min. The bubbles were removed by vacuum and the mixture was injected into a lens mold; ⑶ Place the mold containing the prepolymer in a curing oven at 45°C and heat for 3 hours, then gradually increase the temperature to 85°C and continue to place for 3 hours, and finally cool to room temperature and demold to obtain a high-refractive polyurethane optical material.
[0048] Example 2: Preparation of polyurethane optical material containing tricyclic sulfide compound (i) ⑴ After heating 20g of isothiocyanate compound to 65°C, add 5g of xylene diisocyanate with stirring, and then add 0.4g of triethyldiamine, and stir evenly to obtain a mixture.
[0049] (2) 30 g of the tricyclic sulfide compound (i) prepared above was added to the mixture prepared in step (1), 0.9 g of dibutyltin dilaurate was added to the reaction product, and the mixture was heated to 50°C and stirred for prepolymerization for 35 min. The bubbles were removed by vacuum and the mixture was injected into a lens mold; ⑶ Place the mold containing the prepolymer in a curing oven at 45°C and heat for 3 hours, then gradually increase the temperature to 85°C and continue to place for 3 hours, and finally cool to room temperature and demold to obtain a high-refractive polyurethane optical material.
[0050] Example 3: Preparation of polyurethane optical material containing tricyclic sulfide compound (i) (1) 30 g of the tricyclic sulfide compound (i) prepared above was added to 19 g of xylene diisocyanate and stirred to obtain a reactant.
[0051] (2) Add 0.7 g of dibutyltin dilaurate to the reactant prepared in step (1), heat to 45°C, keep stirring and prepolymerize for 35 min, remove air bubbles in vacuum, and inject into a lens mold; ⑶ Place the mold containing the prepolymer in a curing oven at 45°C and heat for 3 hours, then gradually increase the temperature to 85°C and continue to place for 3 hours, and finally cool to room temperature and demold to obtain a high-refractive polyurethane optical material.
[0052] Example 4: Preparation of polyurethane optical material containing tetracyclic sulfur compound (ii) ⑴ After heating 12g of isothiocyanate compound to 85°C, add 15g of xylene diisocyanate with stirring, and then add 0.2g of triethyldiamine, and stir evenly to obtain a mixture.
[0053] (2) 45 g of the tetracyclic sulfur compound (ii) prepared above was added to the mixture prepared in step (1), 1.1 g of dibutyltin dilaurate was added to the reaction product, and the mixture was heated to 45°C and stirred for prepolymerization for 35 min. The bubbles were removed by vacuum and the mixture was injected into a lens mold; ⑶ Place the mold containing the prepolymer in a curing oven at 45°C and heat for 3 hours, then gradually increase the temperature to 85°C and continue to place for 3 hours, and finally cool to room temperature and demold to obtain a high-refractive polyurethane optical material.
[0054] Example 5: Preparation of polyurethane optical material containing tetracyclic sulfur compound (ii) ⑴ After heating 15g of isothiocyanate compound to 65°C, add 5g of xylene diisocyanate with stirring, and then add 0.4g of triethyldiamine, and stir evenly to obtain a mixture.
[0055] (2) 30 g of the tetracyclic sulfur compound (ii) prepared above was added to the mixture prepared in step (1), 0.9 g of dibutyltin dilaurate was added to the reaction product, and the mixture was heated to 50°C and stirred for prepolymerization for 35 min. The bubbles were removed by vacuum and the mixture was injected into a lens mold; ⑶ Place the mold containing the prepolymer in a curing oven at 45°C and heat for 3 hours, then gradually increase the temperature to 85°C and continue to place for 3 hours, and finally cool to room temperature and demold to obtain a high-refractive polyurethane optical material.
[0056] Example 6: Preparation of polyurethane optical material containing tetracyclic sulfur compound (ii) (1) 45 g of the tetracyclic sulfur compound (ii) prepared above was added to 19 g of xylene diisocyanate and stirred to obtain a reactant; (2) Add 0.7 g of dibutyltin dilaurate to the reactant prepared in step (1), heat to 45°C, keep stirring and prepolymerize for 35 min, remove air bubbles in vacuum, and inject into a lens mold; ⑶ Place the mold containing the prepolymer in a curing oven at 45°C and heat for 3 hours, then gradually increase the temperature to 85°C and continue to place for 3 hours, and finally cool to room temperature and demold to obtain a high-refractive polyurethane optical material.
[0057] Example 7: Preparation of polyurethane optical material containing pentacyclic sulfur compound (iii) ⑴ After heating 20g of isothiocyanate compound to 85°C, add 15g of xylene diisocyanate with stirring, and then add 0.6g of triethyldiamine, and stir evenly to obtain a mixture; (2) 65 g of the pentacyclic sulfur compound (iii) prepared above was added to the mixture prepared in step (1), 1.6 g of dibutyltin dilaurate was added to the reaction product, and the mixture was heated to 45°C and stirred for prepolymerization for 35 min. The bubbles were removed by vacuum and the mixture was injected into a lens mold; ⑶ Place the mold containing the prepolymer in a curing oven at 45°C and heat for 3 hours, then gradually increase the temperature to 85°C and continue to place for 3 hours, and finally cool to room temperature and demold to obtain a high-refractive polyurethane optical material.
[0058] Example 8: Preparation of polyurethane optical material containing pentacyclic sulfur compound (iii) ⑴ After heating 30 g of the pentacyclic sulfur compound (iii) to 50°C, add 15 g of methanedithiol and stir evenly to obtain a mixture; (2) Add the mixture prepared in step (1) above to 20 g of isothiocyanate compound, add 0.6 g of triethyldiamine and 0.9 g of dibutyltin dilaurate to the reactant, heat to 50°C, keep stirring and prepolymerize for 35 min, remove bubbles in vacuum, and inject into a lens mold; ⑶ Place the mold containing the prepolymer in a curing oven at 45°C and heat for 3 hours, then gradually increase the temperature to 85°C and continue to place for 3 hours, and finally cool to room temperature and demold to obtain a high-refractive polyurethane optical material.
[0059] Example 9: Preparation of polyurethane optical material containing pentacyclic sulfur compound (iii) (1) 30 g of the pentacyclic sulfur compound (iii) prepared above was added to 20 g of xylene diisocyanate and stirred to obtain a reactant.
[0060] (2) Add 0.7 g of dibutyltin dilaurate to the reactant prepared in step (1), heat to 45°C, keep stirring and prepolymerize for 35 min, remove air bubbles in vacuum, and inject into a lens mold; ⑶ Place the mold containing the prepolymer in a curing oven at 45°C and heat for 3 hours, then gradually increase the temperature to 85°C and continue to place for 3 hours, and finally cool to room temperature and demold to obtain a high-refractive polyurethane optical material.
[0061] Example 10: Preparation of polyurethane optical material containing pentacyclic sulfur compound (iii) (1) After heating 30 g of the pentacyclic sulfur compound (iii) to 50°C, 0.5 g of toluene solvent was added and stirred to obtain a mixture; (2) After heating 20 g of the isothiocyanate compound to 75° C., 0.3 g of triethyldiamine was added thereto under stirring, and then the mixture prepared in step (1) was added thereto to obtain a reactant; ⑶ Add 0.6 g of dibutyltin dilaurate to the reactant prepared in step (2), heat to 50°C, keep stirring and prepolymerize for 35 min, remove bubbles in vacuo, and inject into a lens mold; (4) Place the mold containing the prepolymer in a curing oven at 45°C and heat for 3 hours, then gradually increase the temperature to 85°C and continue to place for 3 hours, and finally cool to room temperature and demold to obtain a high-refractive polyurethane optical material.
[0062] Example 11: Optical performance testing experiment on polyurethane optical materials The optical properties of the polyurethane optical materials prepared in Examples 1-10 were tested respectively. Light transmittance is one of the most important properties of optical materials, which is expressed by transmittance. The test was performed using the UV-8000 ultraviolet-visible photometer of Shanghai Yuanxi Instrument Co., Ltd. The test method is: directly place the sample on the ultraviolet-visible photometer to measure the transmittance; the refractive index was tested using the WZS1 Abbe refractometer of Shanghai Optical Instrument Equipment Co., Ltd. The test method is: ① dilute the thioether-type episulfide compound prepared in the specific implementation method with ether solvent and apply it on the prism of the Abbe refractometer. After the solvent evaporates, record the test results; ② place the polyurethane optical material samples prepared in Examples 1-10 on the prism of the Abbe refractometer to measure the refractive index. The test results are shown in Figure 5 , Table 1, Table 2.
[0063] Table 1 Refractive index of tested samples Thioether type episulfide compounds i ii iii Refractive index (nd) 1.663 1.712 1.760
[0064] Example 12: Aging resistance test on polyurethane optical materials The polyurethane optical materials prepared in Examples 1-10 were subjected to aging resistance tests respectively. A water-cooled xenon lamp test chamber of Shanghai Diannuo Technology Co., Ltd. was used to select extreme lighting conditions. The samples were irradiated in the aging resistance test chamber for 32 hours. The visible light spectral transmittance (tv) and yellowness index (IY) of the samples were tested before and after irradiation. The test results are shown in Table 3.
[0065]
[0066] Conclusion: Through data comparison, it is known that there is no obvious change in the samples tested in the embodiment.
Claims
1. A high refractive index thioether type episulfide compound, characterized in that: The structure of the compound is shown in Formula I, Formula II or Formula III: Wherein R and R1 are the same or different and are each H, CH3 or C6H5; Wherein R is H or CH3.
2. The method for preparing the high refractive index thioether type episulfide compound I according to claim 1, characterized in that: The method comprises the following steps: (1) 1,3-diphenylacetone and anhydrous ethanol are added to a reaction vessel in a weight ratio of (1-3): (3-7), stirred evenly, and hydrogen sulfide and hydrogen chloride dry gases are introduced successively for 3-7 hours, the reaction temperature is controlled at 0-6° C., and after 10-12 hours, the precipitate is vacuum dried to obtain a thiol intermediate; (2) The thiol intermediate, benzaldehyde and diethyl ether are fully mixed in a weight ratio of (1-2): (1-2): (100-150), and a catalyst in an amount of 1 / 8 to 1 / 12 of the weight of the thiol intermediate is added thereto, and the reaction is stopped after being fully stirred at room temperature for 7-10 hours. A saturated sodium chloride solution is then added, and after stirring and mixing to separate layers, the upper diethyl ether layer is taken out, dried, and decolorized with a concave clay adsorbent until it becomes colorless and transparent, and the diethyl ether solvent is distilled off to obtain a viscous thioether-type tricyclic sulfide compound I.
3. The method for preparing the high refractive index thioether type episulfide compound I according to claim 2, characterized in that: The catalyst is one of hydrochloric acid, sulfuric acid, toluenesulfonic acid and p-toluenesulfonic acid.
4. The method for preparing the high refractive index thioether type episulfide compound II according to claim 1, characterized in that: The method comprises the following steps: (1) 1,3-diphenylacetone and anhydrous ethanol are added to a reaction vessel in a weight ratio of (1-3): (3-7), stirred evenly, and hydrogen sulfide and hydrogen chloride dry gases are introduced successively for 3-7 hours, the reaction temperature is controlled at 0-6° C., and after 10-12 hours, the precipitate is vacuum dried to obtain a thiol intermediate; (2) Add anhydrous ethanol and a thiol intermediate to a reaction vessel. After the thiol intermediate is fully dissolved, add ferric chloride and water. The weight ratio of the thiol intermediate, ethanol, ferric chloride and water is (1-3): (2-5): (2-4): (2-3). Stir the mixture at 0-10° C. for 4-6 hours. A white powdery substance precipitates. Filter the crude product to obtain the crude product. Recrystallize the crude product with n-hexane and dry it in vacuo to obtain a thioether-type tetracyclic sulfur compound II.
5. The method for preparing the high refractive index thioether type episulfide compound III according to claim 1, characterized in that: The method comprises the following steps: adding sodium pentathiocarbonate to methanol, heating to 25-45°C after the mixture is completely dissolved, dripping a dibromomethane methanol solution within 1.5-2.5 hours, and slowly stirring the mixture for reaction for about 30-35 hours; the weight ratio of the sodium pentathiocarbonate, methanol and the dibromomethane methanol solution is (1-3):(2-5):(3-7), and the concentration of the dibromomethane methanol solution is 6-12 wt %; adding distilled water to the reaction system, extracting with chloroform, combining the extracts, and removing the chloroform by atmospheric distillation to obtain a colloidal thioether-type pentacyclic sulfur compound III.
6. The use of the high refractive index thioether type episulfide compound as a polyurethane optical material as claimed in claim 1, characterized in that: The polyurethane optical material is formed by polymerizing the high-refractive-index thioether-type episulfide compound and the isothiocyanate compound and / or the isocyanate compound.
7. The use according to claim 6, characterized in that The mass ratio of the high refractive index thioether type episulfide compound to the isothiocyanate compound, the isocyanate compound or a mixture thereof is (30-70): (10-50).
Citation Information
Patent Citations
Disubstituted tetrathianes as fragrances or flavourings
CN101014586A
Systems, compositions, and methods for corrosion inhibition
CN105189663A
Polyurethane type high-refraction optical resin monomer containing sulfur and preparation method of polyurethane type high-refraction optical resin monomer
CN105777596A
Method for producing 1,2,3,5,6-pentathiepane
CN108633276A
Episulfide compound and composition for optical material
CN112424193A