Anion exchange membrane as well as preparation method and application thereof

By physically blending functionalized hydrogenated styrene-butadiene block copolymers with functionalized organic-inorganic nanomaterials, the problems of insufficient mechanical stability and ionic conductivity of SEBS-based anion exchange membranes were solved, and anion exchange membranes with high ionic conductivity and good dimensional stability were prepared.

CN119039490APending Publication Date: 2024-11-29WEIFANG UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410846925.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In existing anion exchange membrane fuel cells, SEBS-based anion exchange membranes suffer from low ion conductivity, insufficient size and mechanical stability, which affects their application in fuel cells.

Method used

Anion exchange membranes were prepared by physical blending of functionalized hydrogenated styrene-butadiene block copolymers and functionalized organic-inorganic nanomaterials. The rigid cage structure and good compatibility of the functionalized organic-inorganic nanomaterials were utilized to enhance the mechanical properties and ionic conductivity of the polymer.

Benefits of technology

It improves the mechanical stability and ion conductivity of anion exchange membranes, meets the various requirements of fuel cells for anion exchange membranes, and has good dimensional stability and high ion exchange capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039490A_ABST
    Figure CN119039490A_ABST
Patent Text Reader

Abstract

The invention provides a polymer and a functionalized organic-inorganic nano material for preparing an anion exchange membrane, the polymer is prepared by sequentially carrying out functionalization treatment and quaternization reaction on SEBS (Styrene-Ethylene-Butylene-Styrene), and can be used as a skeleton of the anion exchange membrane; according to the functionalized organic-inorganic nano material, 3-chloropropyl trimethoxy silane and concentrated hydrochloric acid are selected to synthesize 3-chloropropyl polyhedral silsesquioxane, and the functionalized organic-inorganic nano material is obtained through quaternization reaction and has a rigid cage-shaped structure. According to the anion exchange membrane prepared by mixing the functionalized organic-inorganic nano material and the polymer, the functionalized organic-inorganic nano material has good compatibility and a rigid cage structure and can be diffused into the polymer to increase the interaction force between molecules, so that the mechanical property of the prepared anion exchange membrane is improved; the formation of a microphase separation structure in the anion exchange membrane is promoted, and the ion exchange capacity and the ion conductivity of the anion exchange membrane are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of anion exchange membrane fuel cells, in particular to polymers and functionalized organic-inorganic nano materials used for preparing anion exchange membranes and anion exchange membranes prepared by using the polymers and functionalized organic-inorganic nano materials. Background Art

[0002] With the growth of global population and economic development, energy demand is increasing, and the pressure of traditional energy consumption and emission is also increasing. Among them, hydrogen energy is regarded as an ideal renewable energy source for human beings in the future due to its high energy density, clean and environmental protection, high calorific value, low loss, storage in various forms, high utilization rate, and convenient transportation. Among many technologies, fuel cells are devices that directly convert the chemical energy of hydrogen and oxygen into electrical energy. They have attracted widespread attention due to their advantages such as high power density, zero emission, and no noise. So far, proton exchange membrane fuel cells (PEMFCs) have been successfully applied in automobiles and other fields. However, the high cost of platinum-based precious metal catalysts and perfluorosulfonic acid membranes has greatly hindered the further development of proton exchange membrane fuel cells. Compared with proton exchange membrane fuel cells, anion exchange membrane fuel cells (AEMFCs) have a great trend of replacing proton exchange membrane fuel cells due to their good operating environment, faster redox reaction kinetics, and the use of non-platinum-based precious metal catalysts. Anion exchange membranes (AEMs) are one of the core components of anion exchange membrane fuel cells. They isolate the anode and cathode gases, provide a transmission channel for OH- in a strong alkaline environment, and prevent fuel penetration from causing internal short circuits in the battery. The performance of AEMs determines the performance of AEMFCs. However, most anion exchange membranes still have the disadvantages of poor chemical stability, insufficient dimensional stability, and low ion conductivity, which cannot meet the requirements of practical applications and large-scale commercialization. Therefore, it is crucial to explore anions with high ion conductivity, excellent chemical stability, stable mechanical properties, and low cost for the commercial application of AEMFCs.

[0003] In terms of chemical structure, it is essentially an ion exchange resin, usually composed of a hydrophobic polymer backbone, hydrophilic cationic groups and freely movable anions. Studies have shown that polymer backbones with electron-withdrawing groups (COC bonds) are degraded by the attack of hydroxide ions in a strong alkaline environment, showing poor chemical stability, while full carbon chain polymer backbones without ether bonds show excellent chemical stability. Therefore, the long-term chemical stability of anion exchange membranes can be improved by selecting full carbon chain polymer backbones without heteroatoms, that is, changing the COC bonds between polymer repeating units to CC bonds.

[0004] Hydrogenated styrene-butadiene block copolymer (SEBS) has the advantages of inherent microphase separation structure, all-carbon chain structure and adjustable soft and hard blocks, and is widely used in anion exchange membranes. However, due to its special fatty chain skeleton structure, SEBS-based anion exchange membranes generally have problems such as low ion conductivity, insufficient dimensional and mechanical stability. Maintaining the good dimensional stability of SEBS-based anion exchange membranes by cross-linking will occupy the sites of grafted cationic groups, thereby inhibiting the ion transport capacity of AMEs; on the other hand, gelation may occur during the cross-linking process, hindering the improvement of the comprehensive performance of AEMs.

[0005] Therefore, designing and preparing a new type of composite anion exchange membrane, improving the mechanical and dimensional stability of SEBS-based anion exchange membrane, broadening the ion transmission channel, and promoting the anion conduction rate have become technical challenges that urgently need to be solved in this technology. Summary of the invention

[0006] The purpose of the present invention is to provide a polymer and a functionalized organic-inorganic nanomaterial for preparing anion exchange membranes and the prepared anion exchange membranes. At the same time, the present invention also provides methods for preparing the same.

[0007] To achieve the above object, in a first aspect, the present invention provides a polymer for preparing anion exchange membrane, wherein the structural formula of the polymer is shown in the following formula (I):

[0008]

[0009] Wherein, R is selected from one of the following structures:

[0010]

[0011] x+y=0.18-0.26, 0<y / (x+y)≤0.74-0.82, a+b=0.74-0.82, m=1 or 6, n1=1~7, n2=1~3.

[0012] In the structural formula (I), x and y together represent the proportion of the styrene block, and the proportion of the entire styrene block accounts for 0.18-0.26 of the total polymer. The reason for distinguishing x and y is that the styrene block is functionalized during the preparation process, and the functionalization includes but is not limited to chloromethylation and acylation. According to the degree of functionalization, 0<y / (x+y)≤0.74-0.82.

[0013] As a preferred embodiment of the polymer of the present invention, in the structural formula (I), x+y+a+b=1.

[0014] As a preferred embodiment of the polymer of the present invention, the polymer is one of the following structural formulas:

[0015]

[0016] In the above structural formula, each bracket represents a block, x+y+a+b=1.

[0017] In a second aspect, the present invention further provides a method for preparing the polymer as described above. To achieve the above object, the technical solution of the present invention is: a method for preparing the polymer as described above for preparing anion exchange membrane, the method comprising the following steps:

[0018] (a1) subjecting a hydrogenated styrene-butadiene block copolymer to a functionalization treatment to obtain a functionalized hydrogenated styrene-butadiene block copolymer capable of undergoing a Menshutkin reaction; the functionalization treatment is an acylation and / or a chloromethylation treatment;

[0019] (a2) reacting the functionalized hydrogenated styrene-butadiene block copolymer obtained in step (a1) with a quaternary ammonium reactant in a solvent to obtain a polymer; the quaternary ammonium reactant is at least one of an alkyl tertiary amine, a six-membered cyclic secondary amine, a spirocyclic secondary amine, and a polycationic side chain.

[0020] As a preferred embodiment of the method for preparing the polymer of the present invention, the functionalization treatment in step (a1) is an acylation treatment, and the acylation comprises the following steps:

[0021] (a1-11) adding a hydrogenated styrene-butadiene block copolymer to a solvent and dissolving it, then adding an acylating agent and a catalyst to react, the reaction temperature is 20-40° C., the reaction time is 5-8 hours, and an acylated product is obtained after the reaction; the acylating agent is 6-bromohexanoyl chloride, and the catalyst is aluminum chloride;

[0022] (a1-12) After purifying the obtained acylation product, mix it with a reducing agent for reduction reaction at a reaction temperature of 50-70°C for a reaction time of 48-60 hours to obtain a functionalized hydrogenated styrene-butadiene block copolymer; the reducing agent is at least one of trifluoroacetic acid and triethylsilane.

[0023] As a preferred embodiment of the method for preparing the polymer of the present invention, when the functionalization treatment in the step (a1) is an acylation treatment, m in the prepared polymer is 6.

[0024] As a preferred embodiment of the method for preparing the polymer of the present invention, the functionalization treatment in step (a1) is a chloromethylation treatment, and the chloromethylation comprises the following steps:

[0025] (a1-2) adding a hydrogenated styrene-butadiene block copolymer to a solvent and dissolving it, then adding a chloromethylation agent and a catalyst to react, the reaction temperature is 0-60°C, the reaction time is 24-72 hours, and after the reaction, a functionalized hydrogenated styrene-butadiene block copolymer is obtained; the chloromethylation agent is at least one of 1,4-dichloromethoxybutane, 1,3,5-trioxane, and trimethylchlorosilane; the catalyst is anhydrous tin tetrachloride.

[0026] As a preferred embodiment of the method for preparing the polymer of the present invention, when the functionalization treatment in the step (a1) is a chloromethylation treatment, m in the prepared polymer is 1.

[0027] As a preferred embodiment of the method for preparing the polymer of the present invention, in the step (a1-11), the mass ratio of the hydrogenated styrene-butadiene block copolymer to the catalyst is 600:1-300:1.

[0028] As a preferred embodiment of the method for preparing the polymer of the present invention, in the step (a1-11), the solvent is at least one of dichloromethane, tetrahydrofuran and chloroform.

[0029] As a preferred embodiment of the method for preparing the polymer of the present invention, in the step (a1-12), the process of purifying the obtained acylated product comprises: pouring the solution after the acylation reaction into a first precipitant for precipitation to obtain a first precipitate; performing a first purification on the first precipitate to obtain the acylated product; the first precipitant is at least one of methanol, petroleum ether and ethanol, and the first purification is: dissolving the first precipitate in dichloromethane and / or tetrahydrofuran and / or chloroform, precipitating it again in the first precipitant, and purifying it.

[0030] As a preferred embodiment of the preparation method of the polymer of the present invention, the product obtained after the reduction reaction in the step (a1-12) is further purified and then subjected to a quaternization reaction. The method of further purifying the product obtained after the reduction reaction includes but is not limited to: neutralizing the acid in the system with the solution obtained after the reduction reaction and the first neutralizer, followed by 2 to 3 extractions, pouring the extracted solution into the second precipitant for precipitation, and then subjecting the precipitated substance to a second purification to obtain the reduced product, which is a functionalized hydrogenated styrene-butadiene block copolymer. The first neutralizer is at least one of sodium bicarbonate, sodium carbonate, and sodium hydroxide, the second precipitant is at least one of ethyl acetate, methanol, and ethanol, and the second purification is: dissolving the precipitated substance in tetrahydrofuran, precipitating it again in the second precipitant, and purifying it.

[0031] As a preferred embodiment of the method for preparing the polymer of the present invention, in the step (a1-2), the mass ratio of the hydrogenated styrene-butadiene block copolymer to the catalyst is 700:1-100:1.

[0032] As a preferred embodiment of the method for preparing the polymer of the present invention, in the step (a1-2), the solvent is at least one of chloroform and tetrahydrofuran.

[0033] As a preferred embodiment of the method for preparing the polymer of the present invention, the product obtained after the reaction in step (a1-2) is further purified and then reacted with the quaternary ammonium product. The method for further purifying the product obtained after the reaction in step (a1-2) includes but is not limited to: adding the solution after the chloromethylation reaction to a third precipitant, and then subjecting the precipitated substance to a third purification to obtain the chloromethylation product. The third precipitant is selected from at least one of methanol and ethanol, and the third purification includes: dissolving the precipitated substance in tetrahydrofuran, precipitating it again in the third precipitant, and purifying it.

[0034] As a preferred embodiment of the preparation method of the polymer of the present invention, the quaternization reactant in step (a2) is at least one of trimethylamine, N,N-dimethylbutylamine, N-methylpiperidine, 3-amino-6-azacyclo[5.5]undecane-6-ammonium bromide, 3-(3-(4-piperidinyl)propyl)-6-azaspiro[5.5]undecane, N,N-dimethyloctylamine, N,N-dimethyldodecylamine, N,N-dimethylhexadecylamine, and 6-dimethylaminohexyltrimethylammonium iodide.

[0035] As a preferred embodiment of the method for preparing the polymer of the present invention, the quaternization reaction temperature in step (a2) is 40-60° C., and the reaction time is 48-72 hours.

[0036] As a preferred embodiment of the method for preparing the polymer of the present invention, the solvent in step (a2) is at least one of chloroform and dichloromethane.

[0037] In a third aspect, the present invention provides a functionalized organic-inorganic nanomaterial for preparing anion exchange membranes, the structural formula of which is shown below:

[0038]

[0039] Wherein, R is selected from one of the following structures:

[0040]

[0041] n1=1~7, n2=1~3.

[0042] In a fourth aspect, the present invention provides a method for preparing the functionalized organic-inorganic nanomaterial as described above, the method comprising the following steps:

[0043] (b1) using 3-chloropropyltrimethoxysilane and concentrated hydrochloric acid as reaction materials and n-butyltin dilaurate as a catalyst, synthesizing 3-chloropropyl polyhedral silsesquioxane by silane self-polymerization in a solvent;

[0044] (b2) reacting the 3-chloropropyl polyhedral silsesquioxane obtained in step (b1) with sodium iodide in a solvent to obtain 3-iodopropyl polyhedral silsesquioxane;

[0045] (b3) reacting the product obtained in step (b2) with a quaternary ammonium reactant in a solvent to obtain a functionalized organic-inorganic nanomaterial;

[0046] The quaternary ammonium reactant in (b3) is at least one of an alkyl tertiary amine (including but not limited to N,N-dimethylbutylamine, N,N-dimethyloctylamine, N,N-dimethyldodecane, N,N-dimethylhexadecane), a six-membered cyclic secondary amine (including but not limited to N-methylpiperidine), a spirocyclic secondary amine (including but not limited to 3-amino-6-azacyclo[5.5]undecane-6-ammonium bromide, 3-(3-(4-piperidinyl)propyl)-6-azaspiro-[5.5]undecane), and a polycationic side chain.

[0047] The functionalized organic-inorganic nanomaterial of the present invention selects 3-chloropropyltrimethoxysilane and concentrated hydrochloric acid to synthesize 3-chloropropyl polyhedral silsesquioxane, and further obtains it through a quaternization reaction. The obtained functionalized organic-inorganic nanomaterial is a functionalized polyhedral silsesquioxane, which has a rigid cage structure and not only has good compatibility, but also can diffuse into the polymer when preparing anion exchange membrane together with the polymer to increase the interaction force between molecules, thereby enhancing the tensile strength of the polymer, thereby achieving the effect of improving the mechanical properties of the anion exchange membrane.

[0048] As a preferred embodiment of the method for preparing functionalized organic-inorganic nanomaterials of the present invention, the concentration of concentrated hydrochloric acid in step (b1) is 36 wt %.

[0049] As a preferred embodiment of the method for preparing the functionalized organic-inorganic nanomaterial of the present invention, the mass ratio of 3-chloropropyltrimethoxysilane to concentrated hydrochloric acid in step (b1) is 200:1-100:1.

[0050] As a preferred embodiment of the method for preparing the functionalized organic-inorganic nanomaterial of the present invention, the mass ratio of 3-chloropropyltrimethoxysilane to the catalyst in step (b1) is 900:1-200:1.

[0051] As a preferred embodiment of the method for preparing functionalized organic-inorganic nanomaterials of the present invention, the dropping speed of concentrated hydrochloric acid in step (b1) is 1-3 seconds / drop, and the dropping speed of 3-chloropropyltrimethoxysilane is 1-3 seconds / drop.

[0052] As a preferred embodiment of the method for preparing the functionalized organic-inorganic nanomaterial of the present invention, the solvent in step (b1) is an anhydrous methanol solution, and the mass ratio of 3-chloropropyltrimethoxysilane to the anhydrous methanol solution is 600:1-300:1.

[0053] As a preferred embodiment of the method for preparing the functionalized organic-inorganic nanomaterials of the present invention, in the step (b1), concentrated hydrochloric acid and 3-chloropropyltrimethoxysilane are first added dropwise to the solvent under ice bath conditions for 30-40 minutes; then the ice bath is removed, the temperature is returned to room temperature and allowed to stand for 2-3 days, and then a catalyst is added and the reaction is carried out at room temperature for 48-60 hours.

[0054] As a preferred embodiment of the method for preparing the functionalized organic-inorganic nanomaterial of the present invention, the 3-chloropropyl polyhedral silsesquioxane obtained in the step (b1) is further purified and then reacted with sodium iodide. The further purification of the 3-chloropropyl polyhedral silsesquioxane includes but is not limited to: the mixture after the reaction in step (b1) is filtered under reduced pressure to obtain a solid substance, and then the precipitated substance is subjected to a fourth purification to obtain a 3-chloropropyl polyhedral silsesquioxane product. The fourth purification includes: washing the precipitated substance with a methanol solution for 2-3 times.

[0055] As a preferred embodiment of the method for preparing functionalized organic-inorganic nanomaterials of the present invention, the solvent in step (b2) is at least one of anhydrous tetrahydrofuran and petroleum ether.

[0056] As a preferred embodiment of the method for preparing the functionalized organic-inorganic nanomaterial of the present invention, the mass ratio of 3-chloropropyl polyhedral silsesquioxane to sodium iodide in step (b2) is 1:10-1:20.

[0057] As a preferred embodiment of the method for preparing the functionalized organic-inorganic nanomaterial of the present invention, the reaction in step (b2) is carried out under light-proof conditions, the reaction temperature is 60-80° C., and the reaction time is 48 to 72 hours.

[0058] As a preferred embodiment of the method for preparing the functionalized organic-inorganic nanomaterial of the present invention, the product after the reaction of 3-chloropropyl polyhedral silsesquioxane and sodium iodide in step (b2) is further purified to obtain 3-iodopropyl polyhedral silsesquioxane, and the method for further purifying the product after the reaction includes but is not limited to: removing the solvent from the reaction mixture by a rotary evaporator to obtain a solid substance, and then subjecting the precipitated substance to a fifth purification to obtain 3-iodopropyl polyhedral silsesquioxane. The fifth purification includes: dissolving the obtained solid in at least one of dichloromethane and chloroform, and removing the solvent again by a rotary evaporator.

[0059] As a preferred embodiment of the method for preparing the functionalized organic-inorganic nanomaterial of the present invention, the reaction in step (b3) needs to be carried out under nitrogen protection.

[0060] As a preferred embodiment of the method for preparing functionalized organic-inorganic nanomaterials of the present invention, the solvent in step (b3) is at least one of anhydrous tetrahydrofuran and petroleum ether.

[0061] As a preferred embodiment of the method for preparing the functionalized organic-inorganic nanomaterials of the present invention, the quaternization reactant in step (b3) is at least one of trimethylamine, N,N-dimethylbutylamine, N-methylpiperidine, N,N-dimethyloctylamine, N,N-dimethyldodecylamine, N,N-dimethylhexadecylamine, and 6-dimethylaminohexyltrimethylammonium iodide.

[0062] As a preferred embodiment of the method for preparing functionalized organic-inorganic nanomaterials of the present invention, the reaction temperature in step (b3) is 60-70° C., and the reaction time is 48-72 hours.

[0063] As a preferred embodiment of the method for preparing the functionalized organic-inorganic nanomaterial of the present invention, the product obtained after the reaction in step (b3) is further purified to obtain the functionalized organic-inorganic nanomaterial, and the method for further purifying the product obtained after the reaction includes but is not limited to: removing the solvent from the mixture after the reaction by a rotary evaporator to obtain a solid substance, and then subjecting the precipitated substance to a sixth purification to obtain the functionalized organic-inorganic nanomaterial. The sixth purification includes: washing the obtained solid substance with tetrahydrofuran 2 to 3 times.

[0064] In a fifth aspect, the present invention further provides an anion exchange membrane, wherein the anion exchange membrane comprises the polymer described above and / or the functionalized organic-inorganic nanomaterial described above.

[0065] As a preferred embodiment of the anion exchange membrane of the present invention, the anion exchange membrane contains the polymer as described above and the functionalized organic-inorganic nanomaterial as described above.

[0066] As a preferred embodiment of the anion exchange membrane of the present invention, the mass percentage of the functionalized organic-inorganic nanomaterial in the anion exchange membrane is 5-20%.

[0067] As a preferred embodiment of the anion exchange membrane of the present invention, the thickness of the anion exchange membrane is 20 to 80 μm.

[0068] In a sixth aspect, the present invention provides a method for preparing the anion exchange membrane as described above, the method comprising the following steps:

[0069] The polymer as described above is dissolved in a solvent, subjected to ultrasonic treatment to obtain a casting solution, and then the casting solution is cast or cast on a substrate, and peeled off after solidification to obtain an anion exchange membrane;

[0070] Alternatively, the polymer as described above is dissolved in a solvent, the functionalized organic-inorganic nanomaterial as described above is added, ultrasonic treatment is performed to obtain a casting solution, and then the casting solution is cast or cast on a substrate, and peeled off after solidification to obtain an anion exchange membrane.

[0071] In the process of preparing the anion exchange membrane of the present invention, the order of preparing the polymer and the functionalized organic-inorganic nanomaterial is not particularly limited. For example, the polymer may be prepared first, or the functionalized organic-inorganic nanomaterial may be prepared first.

[0072] As a preferred embodiment of the method for preparing anion exchange membrane of the present invention, the substrate includes but is not limited to a heat-resistant glass plate, a polytetrafluoroethylene plate, a steel plate, and the like.

[0073] As a preferred embodiment of the method for preparing the anion exchange membrane of the present invention, the prepared anion exchange membrane is immersed in an alkali solution; the alkali solution is an aqueous sodium hydroxide solution and / or an aqueous potassium hydroxide solution, the solubility of the alkali solution is 2-5 mol / L, and the immersion time is 48-72h.

[0074] In a seventh aspect, the present invention further provides an anion exchange membrane fuel cell, wherein the anion exchange membrane fuel cell comprises the polymer as described above;

[0075] and / or, the anion exchange membrane fuel cell comprises the functionalized organic-inorganic nanomaterial as described above;

[0076] Alternatively, the anion exchange fuel cell comprises the anion exchange membrane as described above.

[0077] The polymer of the present invention is a selectively hydrogenated styrene-butadiene block copolymer (SEBS) which is sequentially subjected to functionalization treatment and quaternization reaction. The obtained structural polymer can be used as the skeleton of the anion exchange membrane when used to prepare the anion exchange membrane, and then further forms a physical bond between the added nanomaterial and the polyelectrolyte to improve the thermal stability and mechanical properties of the prepared anion exchange membrane. The present application prepares the nanomaterial into a functionalized organic-inorganic nanomaterial, and forms a specific network structure by physically blending the functionalized organic-inorganic nanomaterial and the polymer. The combination of the full carbon chain structure of the polymer and the advantages of the functionalized organic-inorganic nanomaterial significantly improves the comprehensive performance of the prepared anion exchange membrane.

[0078] When the polymer provided by the present invention is used to prepare an anion exchange membrane, it can be used as a substrate, and when the organic-inorganic nanoparticles are used to prepare an anion exchange membrane, they are mixed with the polymer by physical blending. Since the functionalized organic-inorganic nanomaterials have good compatibility and rigid cage structures, they can diffuse into the polymer to increase the interaction between molecules, thereby enhancing the tensile strength of the matrix, improving the mechanical properties of the prepared anion exchange membrane, promoting the formation of microphase separation structures in the anion exchange membrane, broadening the ion transmission channel, and effectively improving the ion exchange capacity (ICE) and ion conductivity of the anion exchange membrane. The anion exchange membrane provided by the present invention has a uniform and flat surface, adjustable thickness, good dimensional stability, and can meet various requirements of fuel cells for anion exchange membranes.

[0079] The preparation method of the polymer, organic-inorganic nanoparticles and anion exchange membrane provided by the present invention has simple process, readily available raw materials and equipment, and is easy to carry out large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0080] Figure 1 The figure is a schematic structural diagram of an embodiment of the anion exchange membrane of the present invention.

[0081] Figure 2 A preparation flow chart of an embodiment of an anion exchange membrane polymer according to the present invention;

[0082] Figure 3 A preparation flow chart of another embodiment of an anion exchange membrane polymer according to the present invention;

[0083] Figure 4 A flow chart showing the preparation of an embodiment of a functionalized organic-inorganic nanomaterial for anion exchange membrane according to the present invention;

[0084] Figure 5ATR-FTIR spectrum comparison diagram of the functionalized organic-inorganic nanomaterial described in Example 3 of the present invention and the anion exchange membrane described in Examples 4 to 7;

[0085] Figure 6 This is a comparison chart of the ion conductivity of the anion exchange membranes described in Examples 4 to 7 of the present invention.

[0086] Figure 7 This is a comparison diagram of the swelling of the anion exchange membranes described in Examples 4 to 7 of the present invention.

[0087] Figure 8 This is a comparison chart of water absorption of the anion exchange membranes described in Examples 4 to 7 of the present invention. DETAILED DESCRIPTION

[0088] Unless otherwise specified, the raw materials used in the embodiments of the present invention are all conventional raw materials available on the market, the equipment used are all conventional equipment in the technical field, and the methods used are all conventional methods in the technical field. In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments, but it does not constitute any limitation to the protection scope of the present invention. All reasonable changes and combinations included in the scope of the invention spirit of the present invention fall within the protection scope of the present invention.

[0089] The embodiments of the present invention respectively provide a polymer for preparing an anion exchange membrane, a functionalized organic-inorganic nanomaterial, and an anion exchange membrane prepared by using the polymer and the functionalized organic-inorganic nanomaterial.

[0090] The structure of the polymer is shown below:

[0091]

[0092] Wherein, R is selected from one of the following structures:

[0093]

[0094] x+y=0.18-0.26, 0<y / (x+y)≤0.74-0.82, a+b=0.74-0.82, m=1 or 6, n1=1~7, n2=1~3.

[0095] The structure of the functionalized organic-inorganic nanomaterial is as follows:

[0096]

[0097] Wherein, R is selected from one of the following structures:

[0098]

[0099] n1=1~7, n2=1~3.

[0100] When the polymer and the functionalized organic-inorganic nanomaterial are used to prepare an anion exchange membrane, the two are mixed by physical blending. Since the functionalized organic-inorganic nanomaterial has good compatibility and a rigid cage structure, it can diffuse into the polymer to increase the interaction between molecules, and the two can form a specific network structure. The structural schematic diagram of the functionalized organic-inorganic nanomaterial diffused into the polymer is shown in the attached figure. Figure 1 The structure, preparation method and performance of the polymer, functionalized organic-inorganic nanomaterial and anion exchange membrane of the present invention will be further described below in conjunction with specific examples.

[0101] Example 1

[0102] An embodiment of a polymer for anion exchange membrane according to the present invention, wherein the preparation method of the polymer in this embodiment comprises the following steps:

[0103] (a1) Preparation of functionalized hydrogenated styrene-butadiene block copolymer (Br-C6-SEBS)

[0104] (a1-11) Preparation of acyl functionalized hydrogenated styrene-butadiene block copolymer (Br-CO-C6-SEBS): At room temperature, add 150 mL of dichloromethane to a 250 mL round-bottom flask, weigh 5 g of hydrogenated styrene-butadiene block copolymer and add it to the round-bottom flask under stirring. After SEBS is completely dissolved, add 4.46 mL of acylating agent 6-bromohexylamide to the mixed solution, and slowly add 3.89 g of solid anhydrous aluminum chloride as a Lewis acid catalyst, and continue the reaction at room temperature for 5 hours. After the reaction is completed, slowly pour the reacted solution into an excess of methanol solution to precipitate a solid crude product. The obtained solid crude product is dissolved in an appropriate amount of dichloromethane, and then precipitated again with a methanol solution, and a white polymer sample is obtained by vacuum filtration. The sample is placed in a fume hood and dried naturally to obtain an acyl functionalized styrene-butadiene block copolymer (Br-CO-C6-SEBS);

[0105] (a1-12) Preparation of reduced acyl functionalized styrene-butadiene block copolymer (Br-C6-SEBS): At room temperature, 150 mL of dichloromethane was added to a 250 mL round-bottom flask, and 5 g of Br-CO-C6-SEBS obtained in step (a1-11) was weighed and added to the round-bottom flask under stirring. After complete dissolution, 29.23 mL of trifluoroacetic acid and 14.67 mL of triethylsilane were added in sequence, and the mixture was fully reacted at 60° C. for 2 days. The reaction solution was neutralized with an alkaline solution (50 mL of a mixed solution of sodium bicarbonate and sodium hydroxide, both with a concentration of 1 mol / L and a volume ratio of 2:1) to neutrality and extracted 2-3 times. The obtained organic phase solution was poured into excess ethyl acetate for precipitation and purification, and the obtained product was placed in a fume hood and dried naturally at room temperature after reduced pressure filtration to obtain reduced acyl functionalized hydrogenated styrene-butadiene block copolymer (Br-C6-SEBS).

[0106] (a2) Preparation of polymer

[0107] 15mL of chloroform was added to a 50mL round-bottom flask, 0.27g of Br-C6-SEBS obtained in step (a1) was weighed and added to the round-bottom flask under stirring, and after Br-C6-SEBS was completely dissolved, 0.08mL of N-methylpiperidine was added to the reaction to perform quaternary ammonium cation functionalization reaction, and the reaction was continued at 60°C for 48h; after sufficient reaction, the solution after the reaction was slowly poured into excess petroleum ether for precipitation, and repeatedly washed with petroleum ether for 2-3 times, and filtered to obtain a light yellow product. The obtained product was placed in a fume hood and dried naturally to obtain a quaternary ammonium cation functionalized hydrogenated styrene-butadiene block copolymer (Pi-C6-SEBS), which is the polymer described in this embodiment.

[0108] The preparation flow chart of the polymer described in this embodiment is shown in the attached Figure 2 As shown, the structural formula of the polymer prepared in this embodiment is as follows:

[0109]

[0110] Example 2

[0111] An embodiment of a polymer for anion exchange membrane according to the present invention, wherein the preparation method of the polymer in this embodiment comprises the following steps:

[0112] (a1) Preparation of functionalized hydrogenated styrene-butadiene block copolymers

[0113] Preparation of chloromethyl functionalized hydrogenated styrene-butadiene block copolymer (CMSEBS): 120 mL of chloroform and 4 g of hydrogenated styrene-butadiene block copolymer were added to a 250 mL three-necked flask, and the reaction temperature was raised to 55°C after stirring and dissolving. 16.8 mL of 1,4-dichloromethylbutane and 2.4 mL of anhydrous tin tetrachloride were slowly added to the flask at a rate of 1 second / drop, and the reaction was carried out at 55°C for 5 hours. After the reaction was complete, the solution was slowly poured into 300 mL of methanol for precipitation, and a light purple solid crude product was obtained by a vacuum filtration device. The crude product was then dissolved in 100 mL of tetrahydrofuran for purification, and then precipitated again with methanol, and this was repeated 2-3 times. The obtained product was placed in a fume hood and dried naturally, and the obtained milky white solid was the preparation of chloromethyl functionalized hydrogenated styrene-butadiene block copolymer (CMSEBS).

[0114] (a2) Preparation of polymer

[0115] 15 mL of chloroform was added to a 50 mL round-bottom flask, 0.27 g of the CMSEBS obtained in step (a1) was weighed and added to the round-bottom flask under stirring. After the CMSEBS was completely dissolved, 0.1 mL of N, N-dimethylhexadecylamine was added to the single-necked flask, and the reaction was continued at 60° C. for 48 hours; after sufficient reaction, the solution after the reaction was slowly poured into an excess of petroleum ether for precipitation, and repeatedly washed with petroleum ether for 2-3 times, and filtered to obtain a light yellow product. The obtained product was placed in a fume hood and dried naturally to obtain a quaternary ammonium cation functionalized hydrogenated styrene-butadiene block copolymer (C16-SEBS), which is the polymer described in this embodiment.

[0116] The preparation flow chart of the polymer described in this embodiment is shown in the attached Figure 3 As shown, the structural formula of the polymer prepared in this embodiment is as follows:

[0117]

[0118] Example 3

[0119] An embodiment of a functionalized organic-inorganic nanomaterial for an anion exchange membrane according to the present invention, wherein the method for preparing the functionalized organic-inorganic nanomaterial in this embodiment comprises the following steps:

[0120] (b1) Preparation of 3-chloropropyl polyhedral silsesquioxane (Cl-POSS): 120 mL of anhydrous methanol was added to a single-necked flask. After 20 minutes of treatment under ice bath conditions, 5 ml of concentrated hydrochloric acid was slowly added dropwise to the anhydrous methanol at a rate of 1 second / drop. Subsequently, 3-chloropropyltrimethoxysilane was slowly added dropwise to the single-necked flask at a rate of 1 second / drop. The ice bath was removed after 30 minutes of continuous ice bathing. The reaction returned to room temperature and was left to stand for 2 days to completely hydrolyze the methoxy groups in the reactant. After the hydrolysis was complete, 0.1 g of n-butyltin dilaurate was added to catalyze the initiation of silane self-polymerization reaction. The reaction was continued at room temperature for 48 hours, and a white solid was gradually precipitated during the reaction. After the reaction was completed, the white solid product was obtained by vacuum filtration, and washed 2-3 times with methanol. After vacuum drying, 3-chloropropyl polyhedral silsesquioxane (Cl-POSS) was obtained.

[0121] (b2) Preparation of 3-iodopropyl polyhedral silsesquioxane (I-POSS): 200 mL of anhydrous tetrahydrofuran was added to a single-necked flask, followed by 2 g of Cl-POSS, and after stirring and dissolving, a light shielding device was assembled; then 0.4 g / mL of sodium iodide acetone solution was slowly added dropwise, a reflux device was assembled, and the reaction was carried out at 75°C for 48 hours. After the reaction was complete, a pale yellow solid crude product was obtained by rotary evaporation. The crude product was redissolved in 80 mL of dichloromethane, and the insoluble matter was removed by vacuum filtration. The resulting clear liquid was subjected to rotary evaporation to obtain the product, and after vacuum drying, 3-iodopropyl polyhedral silsesquioxane (I-POSS) was obtained.

[0122] (b3) Preparation of N,N-dimethylbutylamine quaternary ammonium functionalized polyhedral silsesquioxane (C4-POSS): 20 mL of anhydrous tetrahydrofuran was added to a single-necked flask, and the mixture was evacuated. 1 g of I-POSS was added under nitrogen protection, and 0.46 mL of N,N-dimethylbutylamine was added dropwise, and the mixture was reacted at 60° C. for 72 hours. After the reaction was complete, a pale yellow solid crude product was obtained by rotary evaporation, which was washed with tetrahydrofuran 2-3 times and then dried in vacuum to obtain N,N-dimethylbutylamine quaternary ammonium functionalized polyhedral silsesquioxane (C4-POSS), which is the functionalized organic-inorganic nanomaterial described in this embodiment.

[0123] The preparation flow chart of the functionalized organic-inorganic nanomaterials described in this embodiment is shown in the attached figure. Figure 4 As shown, the structural formula of the functionalized organic-inorganic nanomaterial prepared in this embodiment is as follows:

[0124]

[0125] Example 4

[0126] An embodiment of the anion exchange membrane of the present invention is prepared by the following method:

[0127] The polymer quaternary ammonium cation functionalized hydrogenated styrene-butadiene block copolymer (Pi-C6-SEBS) prepared in Example 1 was dissolved in an appropriate amount of chloroform, and ultrasonically treated to obtain a homogeneous casting solution. The casting solution was poured into a flat-bottomed surface dish to form a film, and then placed in a fume hood to allow the solvent to evaporate naturally to form a film. The film was then peeled off to obtain a composite anion exchange membrane. The obtained membrane was immersed in a 1M NaOH solution to obtain OH - The anion exchange membrane in the form of (Pi-C6-SEBS) is the anion exchange membrane described in this embodiment.

[0128] Example 5

[0129] An embodiment of the anion exchange membrane of the present invention is prepared by the following method:

[0130] The polymer quaternary ammonium cation functionalized hydrogenated styrene-butadiene block copolymer (Pi-C6-SEBS) prepared in Example 1 was dissolved in an appropriate amount of chloroform to obtain a homogeneous solution; the functionalized organic-inorganic nanomaterial C4-POSS prepared in Example 3 was dissolved in an appropriate amount of chloroform, then added to the Pi-C6-SEBS solution, and ultrasonically treated to obtain a homogeneous casting solution, and the obtained casting solution was poured into a flat-bottomed surface dish to cast a film, placed in a fume hood to allow the solvent to evaporate naturally to form a film, and then the film was peeled off to obtain a composite anion exchange membrane. The obtained membrane was immersed in a 1M NaOH solution to obtain OH - The anion exchange membrane in the form of (C4-POSS-Pi-C6-SEBS) is the anion exchange membrane described in this embodiment.

[0131] Example 6

[0132] An embodiment of the ion exchange membrane of the present invention, the anion exchange membrane described in this embodiment is prepared by the following method:

[0133] The polymer quaternary ammonium cation functionalized hydrogenated styrene-butadiene block copolymer (C16-SEBS) prepared in Example 2 was dissolved in an appropriate amount of chloroform, and ultrasonically treated to obtain a homogeneous casting solution. The casting solution was poured into a flat-bottomed surface dish to form a film, and the film was placed in a fume hood to allow the solvent to evaporate naturally to form a film, and then the film was peeled off to obtain a composite anion exchange membrane. The obtained membrane was immersed in a 1M NaOH solution to obtain an anion exchange membrane (C16-SEBS) in the OH- form, which is the anion exchange membrane described in this embodiment.

[0134] Example 7

[0135] An embodiment of the ion exchange membrane of the present invention, the anion exchange membrane described in this embodiment is prepared by the following method:

[0136] The polymer quaternary ammonium cation functionalized hydrogenated styrene-butadiene block copolymer (C16-SEBS) prepared in Example 2 was dissolved in an appropriate amount of chloroform to obtain a homogeneous solution; the functionalized organic-inorganic nanomaterial C4-POSS prepared in Example 3 was dissolved in an appropriate amount of chloroform, then added to the C16-SEBS solution, and ultrasonically treated to obtain a homogeneous casting solution, and the obtained casting solution was poured into a flat-bottomed surface dish to cast a film, placed in a fume hood to allow the solvent to evaporate naturally to form a film, and then the film was peeled off to obtain a composite anion exchange membrane. The obtained membrane was immersed in a 1M NaOH solution to obtain OH - The anion exchange membrane in the form of (C4-POSS-C16-SEBS) is the anion exchange membrane described in this embodiment.

[0137] Example 8

[0138] Performance test of the anion exchange membrane of the present invention

[0139] (1) Fourier transform infrared (ATR-FTIR) spectroscopy test

[0140] The Fourier transform infrared (ATR-FTIR) spectra of Examples 3 to 7 were measured using a Nicolet 6700 spectrometer in the wave number range of 3700-700 cm-1. The test results are as follows: Figure 5 As shown. Figure 5 It can be seen that the peak at 1250cm-1 in the infrared spectrum of C4-POSS is the stretching vibration peak of -N+R3, and 1090cm-1 is the stretching vibration peak at Si-O-Si, confirming the successful synthesis of C4-POSS. It can be seen from the infrared spectra of Examples 4 to 7 that the stretching vibration peaks at 2948cm-1 and 2860cm-1 are the stretching vibration peaks of -CH2- in the hydrogenated styrene-butadiene block copolymer, the peak at 1250cm-1 is the stretching vibration peak of -N+R3, and 3439cm-1 is the stretching vibration peak of -OH, confirming the successful synthesis of the quaternary ammonium functionalized hydrogenated styrene-butadiene block copolymer.

[0141] (2) Test of Hydroxide Ion Conductivity

[0142] The anion exchange membranes of Examples 4 to 7 of the present invention were tested for hydroxyl ion conductivity at different temperatures using a two-electrode alternating current impedance method using an electrochemical workstation (Zahner Ennium). Figure 6As shown, with the increase of temperature, the ion conduction of the anion exchange membrane in the embodiments 4 to 7 is significantly improved. After adding functionalized C4-POSS, due to the presence of tightly packed cation exchange groups in the composite membrane, the hydrophilic cationic groups and hydrophobic core contained in C4-POSS promote the hydrophilic / hydrophobic phase separation in the membrane, respectively, and help to build interconnected OH-transmission channels in the membrane, so that the ion conductivity of the composite anion exchange membrane of embodiments 5 and 7 is significantly higher than that of embodiments 4 and 6, and it can be seen that C4-POSS nanoparticles play a good role in the transmission of OH-. At 80 ° C, the ion conductivity of embodiments 4 to 7 can reach 70.6mS / cm, 84.9mS / cm, 60.5mS / cm, and 80.1mS / cm, respectively, which all meet the requirements of the anion exchange membrane of fuel cells at this stage for ion conductivity.

[0143] (3) Swelling test

[0144] The anion exchange membranes of Examples 4 to 7 were subjected to swelling tests. The dry membrane samples in the OH- form were immersed in deionized water. After reaching water absorption equilibrium at different temperatures, the moisture on the surface of the membrane samples was wiped off with filter paper. The length L1 of the wet membrane samples at different temperatures was measured. The membrane samples were then placed under vacuum drying at 60°C for 48 hours, and the length L2 of the dry membrane was measured. The swelling (SR) calculation formula of the membrane samples at different temperatures is as follows:

[0145]

[0146] The relationship between the swelling and temperature of the anion exchange membranes prepared in Examples 4 to 7 is shown in the attached figure. Figure 7 As shown in the attached Figure 7 As shown, the swelling of the anion exchange membrane increases with the increase of temperature, which is due to the acceleration of ion movement at high temperature. Since the presence of the Si-O-Si and O-Si-O hydrophobic cores in C4-POSS reduces the hydrophilicity, the swelling rate of the composite anion exchange membranes of Examples 5 and 7 is lower than that of the membranes of Examples 4 and 6, indicating that the addition of organic-inorganic nanoparticles is beneficial to improving the dimensional stability of the composite anion exchange membrane.

[0147] (4) Water absorption test

[0148] The anion exchange membranes of Examples 4 to 7 were subjected to swelling tests. The membrane samples in the OH- form with a size of 2 cm×2 cm were cut, soaked in the specified constant temperature distilled water for 5 hours, taken out, and the water was absorbed. The wet weight m1 was recorded, and then the membrane samples were placed in a 60°C vacuum oven to be thoroughly dried, and the dry weight m2 was recorded. The water absorption (WU) of the membrane samples at different temperatures was calculated as follows:

[0149]

[0150] The relationship between water absorption and temperature of the anion exchange membranes prepared in Examples 4 to 7 is shown in the attached figure. Figure 8 As shown in Figure 2, the water absorption of the prepared anion exchange membrane increases with the increase of temperature, and the water absorption of the composite anion exchange membrane after adding C4-POSS is significantly reduced, indicating that the rigid cage structure of C4-POSS can effectively prevent excessive water swelling.

[0151] Based on the above content, it can be seen that the anion exchange membrane of the present invention has good ion conductivity, especially the composite anion exchange membrane prepared by the polymer and the functionalized organic-inorganic nanomaterial, which not only maintains good dimensional stability but also has high ion conductivity. This is attributed to the addition of functionalized organic-inorganic nanoparticles, which promotes the generation of microphase separation in the membrane. At the same time, the presence of the rigid cage structure reduces the swelling and water absorption of the anion exchange membrane, and the presence of the cationic functionalized group promotes the transmission of OH-.

[0152] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A polymer for preparing anion exchange membrane, characterized in that The structural formula of the polymer is shown in the following formula (I): Wherein, R is selected from one of the following structures: x+y=0.18-0.26, 0<y / (x+y)≤0.74-0.82, a+b=0.74-0.82, m=1 or 6, n1=1~7, n2=1~3.

2. The polymer for preparing anion exchange membrane according to claim 1, characterized in that The polymer is one of the following structural formulas:

3. A method for preparing a polymer for preparing anion exchange membrane as claimed in any one of claims 1 to 2, characterized in that: The method comprises the following steps: (a1) subjecting a hydrogenated styrene-butadiene block copolymer to a functionalization treatment to obtain a functionalized hydrogenated styrene-butadiene block copolymer capable of undergoing a Menshutkin reaction; the functionalization treatment is an acylation and / or a chloromethylation treatment; (a2) reacting the functionalized hydrogenated styrene-butadiene block copolymer obtained in step (a1) with a quaternary ammonium reactant in a solvent to obtain a polymer; the quaternary ammonium reactant is at least one of an alkyl tertiary amine, a six-membered cyclic secondary amine, a spirocyclic secondary amine, and a polycationic side chain.

4. The method for preparing a polymer for preparing anion exchange membrane according to claim 3, characterized in that: The functionalization treatment in step (a1) is an acylation treatment, and the acylation comprises the following steps: (a1-11) adding a hydrogenated styrene-butadiene block copolymer to a solvent and dissolving it, then adding an acylating agent and a catalyst to react, the reaction temperature is 20-40° C., the reaction time is 5-8 hours, and an acylated product is obtained after the reaction; the acylating agent is 6-bromohexanoyl chloride, and the catalyst is aluminum chloride; (a1-12) purifying the obtained acylated product and mixing it with a reducing agent for reduction reaction at a reaction temperature of 50-70° C. for a reaction time of 48-60 h to obtain a functionalized hydrogenated styrene-butadiene block copolymer; the reducing agent is at least one of trifluoroacetic acid and triethylsilane; Alternatively, the functionalization treatment in step (a1) is a chloromethylation treatment, and the chloromethylation comprises the following steps: (a1-2) adding a hydrogenated styrene-butadiene block copolymer to a solvent and dissolving it, then adding a chloromethylation agent and a catalyst to react, the reaction temperature is 0-60° C., the reaction time is 24-72 hours, and after the reaction, a functionalized hydrogenated styrene-butadiene block copolymer is obtained; the chloromethylation agent is at least one of 1,4-dichloromethoxybutane, 1,3,5-trioxane, and trimethylchlorosilane; the catalyst is anhydrous tin tetrachloride; Preferably, in the step (a1-11), the mass ratio of the hydrogenated styrene-butadiene block copolymer to the catalyst is 600:1-300:1; And / or, preferably, in the step (a1-11), the solvent is at least one of dichloromethane, tetrahydrofuran and chloroform; And / or, preferably, in the step (a1-12), the process of purifying the obtained acylated product comprises: pouring the solution after the acylation reaction into a first precipitant for precipitation to obtain a first precipitate; performing a first purification on the first precipitate to obtain the acylated product; the first precipitant is at least one of methanol, petroleum ether and ethanol, and the first purification comprises: dissolving the first precipitate in dichloromethane and / or tetrahydrofuran and / or chloroform, and precipitating it again in the first precipitant for purification; And / or, preferably, in the step (a1-2), the mass ratio of the hydrogenated styrene-butadiene block copolymer to the catalyst is 700:1-100:1; And / or, preferably, in the step (a1-2), the solvent is at least one of chloroform and tetrahydrofuran.

5. The method for preparing a polymer for preparing an anion exchange membrane according to claim 3, characterized in that: In step (a2), the quaternization reactant is at least one of trimethylamine, N,N-dimethylbutylamine, N-methylpiperidine, 3-amino-6-azacyclo[5.5]undecane-6-ammonium bromide, 3-(3-(4-piperidinyl)propyl)-6-azaspiro[5.5]undecane, N,N-dimethyloctylamine, N,N-dimethyldodecylamine, N,N-dimethylhexadecylamine, and 6-dimethylaminohexyltrimethylammonium iodide; And / or, in step (a2), the quaternization reaction temperature is 40-60° C., and the reaction time is 48-72 h; And / or, the solvent in step (a2) is at least one of chloroform and dichloromethane.

6. A functionalized organic-inorganic nanomaterial for preparing anion exchange membrane, characterized in that: Its structural formula is as follows: Wherein, R is selected from one of the following structures: n1=1~7, n2=1~3.

7. The method for preparing a functionalized organic-inorganic nanomaterial for preparing anion exchange membrane according to claim 6, characterized in that: The method comprises the following steps: (b1) using 3-chloropropyltrimethoxysilane and concentrated hydrochloric acid as reaction materials and n-butyltin dilaurate as a catalyst, synthesizing 3-chloropropyl polyhedral silsesquioxane by silane self-polymerization in a solvent; (b2) reacting the 3-chloropropyl polyhedral silsesquioxane obtained in step (b1) with sodium iodide in a solvent to obtain 3-iodopropyl polyhedral silsesquioxane; (b3) reacting the product obtained in step (b2) with a quaternary ammonium reactant in a solvent to obtain a functionalized organic-inorganic nanomaterial; The quaternary ammonium reactant in (b3) is at least one of an alkyl tertiary amine (including but not limited to N,N-dimethylbutylamine, N,N-dimethyl-n-octylamine, N,N-dimethyldodecane, N,N-dimethylhexadecane), a six-membered cyclic secondary amine (including but not limited to N-methylpiperidine), a spirocyclic secondary amine (including but not limited to 3-amino-6-azacyclo[5.5]undecane-6-ammonium bromide, 3-(3-(4-piperidinyl)propyl)-6-azaspiro-[5.5]undecane), and a polycationic side chain; Preferably, the concentration of concentrated hydrochloric acid in step (b1) is 36wt%; And / or, preferably, in step (b1), the mass ratio of 3-chloropropyltrimethoxysilane to concentrated hydrochloric acid is 200:1-100:1; And / or, preferably, in step (b1), the mass ratio of 3-chloropropyltrimethoxysilane to the catalyst is 900:1-200:1; And / or, preferably, in step (b1), the dropping speed of concentrated hydrochloric acid is 1-3 seconds / drop, and the dropping speed of 3-chloropropyltrimethoxysilane is 1-3 seconds / drop; And / or, preferably, the solvent in step (b1) is an anhydrous methanol solution, and the mass ratio of 3-chloropropyltrimethoxysilane to the anhydrous methanol solution is 600:1-300:1; And / or, preferably, in the step (b1), concentrated hydrochloric acid and 3-chloropropyltrimethoxysilane are first added dropwise to the solvent under ice bath conditions for 30-40 minutes; then the ice bath is removed, the temperature is returned to room temperature and allowed to stand for 2-3 days, and then a catalyst is added and the reaction is carried out at room temperature for 48-60 hours; And / or, preferably, the solvent in step (b2) is at least one of anhydrous tetrahydrofuran and petroleum ether; And / or, preferably, the mass ratio of 3-chloropropyl polyhedral silsesquioxane to sodium iodide in step (b2) is 1:10-1:20; And / or, preferably, the reaction in step (b2) is carried out under light-proof conditions, the reaction temperature is 60-80° C., and the reaction time is 48-72 h; And / or, preferably, the step (b3) needs to be reacted under nitrogen protection; And / or, preferably, the solvent in step (b3) is at least one of anhydrous tetrahydrofuran and petroleum ether; And / or, preferably, the quaternization reactant in step (b3) is at least one of trimethylamine, N,N-dimethylbutylamine, N-methylpiperidine, N,N-dimethyloctylamine, N,N-dimethyldodecylamine, N,N-dimethylhexadecylamine, and 6-dimethylaminohexyltrimethylammonium iodide; And / or, preferably, the reaction temperature in step (b3) is 60-70°C, and the reaction time is 48-72h.

8. An anion exchange membrane, characterized in that: The anion exchange membrane contains the polymer as claimed in claims 1 to 2 and / or the functionalized organic-inorganic nanomaterial as claimed in claim 6; preferably, the anion exchange membrane contains the polymer and the functionalized organic-inorganic nanomaterial; Preferably, the mass percentage of the functionalized organic-inorganic nanomaterial in the anion exchange membrane is 5 to 20%; And / or, preferably, the anion exchange membrane has a thickness of 20 to 80 μm.

9. A method for preparing an anion exchange membrane as claimed in claim 8, characterized in that: The method comprises the following steps: The polymer as claimed in claim 1 to 2 is dissolved in a solvent, subjected to ultrasonic treatment to obtain a casting solution, and then the casting solution is cast or cast on a substrate, and peeled off after solidification to obtain an anion exchange membrane; Alternatively, the polymers as claimed in claims 1 to 2 are dissolved in a solvent, the functionalized organic-inorganic nanomaterials as claimed in claim 7 are added, ultrasonic treatment is performed to obtain a casting solution, and then the casting solution is cast or cast on a substrate, and peeled off after solidification to obtain an anion exchange membrane.

10. An anion exchange membrane fuel cell, characterized in that: The anion exchange membrane fuel cell comprises the polymer according to any one of claims 1 to 2; and / or, the anion exchange membrane fuel cell comprises the functionalized organic-inorganic nanomaterial as claimed in claim 6; Or, the anion exchange fuel cell comprises the anion exchange membrane according to any one of claims 8.

Citation Information

Cited By

  • An anion exchange membrane containing short-chain 6,6-spirocyclic piperidine quaternary ammonium salt units and a preparation method and application thereof