Conjugated polymer based on fluorine-containing acenaphtho quinoxaline condensed ring unit and preparation method and application thereof
By designing a conjugated polymer based on fluorine-containing acetonoxaline thick ring unit, the problems of fewer types of organic solar cell materials and low open circuit voltage in the prior art are solved, and a wide optical absorption range and deep energy level are achieved, thereby improving the The device performance and synthesis simplicity are achieved, with an open circuit voltage of 12.8%.
Patent Information
- Application Number
- CN202411166289.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing high-efficiency binary organic solar cells have fewer types of active layer materials, low open circuit voltage and complex synthesis, especially polymer donor materials, which show poor device performance.
A conjugated polymer based on fluoroquinoxaline-containing fused ring units was designed to achieve a wide optical absorption range and depth by adjusting the type of electron donation units in D-A polymer and the length of alkyl chains on the thiophene bridge. The highest occupies the molecular orbital energy level and provides a method for preparing the conjugated polymer.
It achieves a wide optical absorption range, the highest deep occupancy of molecular orbital energy level and good thermal stability, improves the performance of organic solar cells, the open circuit voltage can reach 12.8%, and simplifies the synthesis and purification process and improves the yield.
Smart Images

Figure CN119039573A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of new energy battery materials, and more specifically, to a conjugated polymer based on a fluorinated acenaphthene-quinoxaline fused ring unit and a preparation method and application thereof. Background Art
[0002] With the continuous consumption of non-renewable energy, solar energy is a stable source all over the world, which is undoubtedly the first choice for green energy development. Organic solar cells (OSCs) that use organic photoactive materials to absorb sunlight and convert it into electrical energy have attracted widespread attention from academia and industry around the world in recent decades, thanks to their significant advantages such as low cost, inherent flexibility, light weight, and strong solution processing capabilities. With the innovation of active layer materials and device processing, the power conversion efficiency of single-junction organic solar cells has been improved to more than 19%.
[0003] At present, the active layer of most efficient binary OSCs is usually composed of DA-type polymer donors and A-DA'DA-type non-fullerene acceptors (NFAs). The emergence of Y-series NFAs has greatly promoted the development of OSCs. In contrast, efficient polymer donors have lagged behind. Despite the emergence of many innovative polymer donor materials, PM6 and D18 are still the most widely used and representative polymer donors. Inefficient polymer donors often show poor device performance and low open-circuit voltage. This requires the rational design of molecular structure. It is still a huge challenge to further realize efficient donor materials through innovative molecular design.
[0004] Application Contents
[0005] In order to overcome at least one problem existing in the prior art, the primary purpose of the present application is to provide a conjugated polymer based on a fluorinated acenaphthene-quinoxaline fused ring unit, which can solve the problems of relatively few types of existing high-efficiency polymer donor materials, low open circuit voltage and relatively complex synthesis.
[0006] The second object of the present application is to provide a method for preparing the above-mentioned conjugated polymer based on fluorine-containing acenaphthene-quinoxaline fused ring units.
[0007] The third object of the present application is to provide the application of the above-mentioned conjugated polymer based on fluorinated acenaphthene-quinoxaline fused ring unit. The present application achieves a wide optical absorption range and a deep highest occupied molecular orbital (HOMO) energy level by adjusting the type of electron-donating unit in the DA polymer and the length of the alkyl chain on the thiophene bridge, while obtaining higher device performance.
[0008] To achieve the above objectives, this application provides the following solutions:
[0009] The present application provides a conjugated polymer based on a fluorinated acenaphthene-quinoxaline fused ring unit. The structure of the conjugated polymer based on a fluorinated acenaphthene-quinoxaline fused ring unit is shown in the general formula (I):
[0010]
[0011] Wherein, n is the degree of polymerization, which is a natural number selected from 1 to 100, D is the electron donating unit, R 1 and R 2 is independently selected from hydrogen, fluorine, and carbon atoms C 1 ~C 100 Any of a straight chain alkyl group or a branched chain alkyl group, an alkoxy group or a sulfanyl group, R 3 It is hydrogen or cyano.
[0012] Preferably, the electron donating group has any one of the following molecular structural formulas:
[0013]
[0014] Preferably, the degree of polymerization n is a natural number between 1 and 50.
[0015] More preferably, the conjugated polymer based on fluorinated acenaphthene-quinoxaline fused ring units is selected from any one of the following structural formulas:
[0016]
[0017] The present application also provides a method for preparing the above-mentioned conjugated polymer based on fluorinated acenaphthene-quinoxaline fused ring units, comprising the following steps:
[0018] S1. Synthesis of intermediates A1 and A2
[0019] S11. 8,11-dibromo-9,10-difluoroacenaphtho[1,2-b]quinoxaline and tributyl(4-(2-ethylhexyl)thiophen-2-yl)stannane are reacted under the catalysis of tetrakis(triphenylphosphine)palladium to obtain 8,11-bis(4-(2-ethylhexyl)thiophen-2-yl)-9,10-difluoroacenaphtho[1,2-b]quinoxaline A1;
[0020] S12. 8,11-dibromo-9,10-difluoroacenaphtho[1,2-b]quinoxaline and tributyl(4-(2-octyldecyl)thiophen-2-yl)stannane are reacted under the catalysis of tetrakis(triphenylphosphine)palladium to obtain 8,11-bis(4-(2-octyldecyl)thiophen-2-yl)-9,10-difluoroacenaphtho[1,2-b]quinoxaline A2;
[0021] S2. Synthesis of monomers M1 and M2
[0022] S21. A1 in step S11 is reacted with N-bromosuccinimide to obtain 8,11-bis(5-bromo-4-(2-ethylhexyl)thiophen-2-yl)-9,10-difluoroacenaphtho[1,2-b]quinoxaline M1;
[0023] S22. A2 in step S12 is reacted with N-bromosuccinimide to obtain 8,11-bis(5-bromo-4-(2-octyldecyl)thiophen-2-yl)-9,10-difluoroacenaphtho[1,2-b]quinoxaline M2;
[0024] S3. Synthetic polymers P1 to P4
[0025] S31. M1 in step S21 is reacted with (4,8-bis(4-(2-ethylhexyl)-5-fluorothiophen-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) in the presence of tri(dibenzylideneacetone)dipalladium and tri(o-methylphenyl)phosphine using chlorobenzene as solvent, and the polymer P1 is obtained by Soxhlet extraction;
[0026] S32. M1 in step S21 is reacted with (4,8-bis(4-(2-ethylhexyl)-5-chlorothiophene-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) in the presence of tri(dibenzylideneacetone)dipalladium and tri(o-methylphenyl)phosphine using chlorobenzene as solvent, and the polymer P2 is obtained by Soxhlet extraction;
[0027] S33. The M2 in step S22 is reacted with (4,8-bis(4-(2-ethylhexyl)-5-fluorothiophen-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) in the presence of tri(dibenzylideneacetone)dipalladium and tri(o-methylphenyl)phosphine using chlorobenzene as solvent, and the polymer P3 is obtained by Soxhlet extraction;
[0028] S34. The M2 in step S22 is reacted with (4,8-bis(4-(2-ethylhexyl)-5-chlorothiophene-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethyltinane) in the presence of tri(dibenzylideneacetone)dipalladium and tri(o-methylphenyl)phosphine using chlorobenzene as solvent, and the polymer P4 is obtained by Soxhlet extraction.
[0029] Preferably, the molar ratio of 8,11-dibromo-9,10-difluoroacenaphtho[1,2-b]quinoxaline, tributyl(4-(2-ethylhexyl)thiophen-2-yl)stannane and tetrakis(triphenylphosphine)palladium catalyst in step S11 is 1:(2.1-2.2):(0.05-0.0.07).
[0030] Preferably, in step S12, the molar ratio of 8,11-dibromo-9,10-difluoroacenaphtho[1,2-b]quinoxaline, tributyl(4-(2-octyldecyl)thiophen-2-yl)stannane and tetrakis(triphenylphosphine)palladium catalyst is 1:(2.1-2.2):(0.05-0.0.07).
[0031] Preferably, the reaction in step S1 is carried out in an organic solvent under nitrogen protection, the reaction temperature is 120-130° C., and the reaction time is 8-12 h.
[0032] Preferably, in step S2, the molar ratio of A1 to N-bromosuccinimide is 1:(2.0-2.1); the molar ratio of A2 to N-bromosuccinimide is 1:(2.0-2.1); the reaction is carried out in an organic solvent and under nitrogen protection, at room temperature in the dark, and the reaction time is 2-4 hours.
[0033] Preferably, in step S3, the molar ratio of M1 to (4,8-bis(4-(2-ethylhexyl)-5-fluorothiophene-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) is 1:1; the molar ratio of M1 to (4,8-bis(4-(2-ethylhexyl)-5-chlorothiophene-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) is 1:1; the molar ratio of M2 to (4,8-bis(4-(2-ethylhexyl)-5-fluorothiophene- The molar ratio of M2 and (4,8-bis(4-(2-ethylhexyl)-5-chlorothiophene-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethyltinane) is 1:1; the molar ratio of M2 and (4,8-bis(4-(2-ethylhexyl)-5-chlorothiophene-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethyltinane) is 1:1; the reaction is carried out in the dark under nitrogen protection, the mass of tri(dibenzylideneacetone)dipalladium is 6-8 mg, the mass of tri(o-methylphenyl)phosphine is 12-16 mg, and the reaction time is 48 h.
[0034] More preferably, after the reaction described in step S3 is completed, the mixture is cooled to room temperature and precipitated with methanol, and then purified by a Soxhlet extractor with methanol, petroleum ether, dichloromethane and chloroform to remove oligomers and residual catalysts, and then the solution is evaporated and concentrated, and precipitated into a methanol solution, and finally the solid is collected by filtration and dried in a vacuum to obtain a conjugated polymer based on a fluorinated acenaphthene-quinoxaline fused ring unit.
[0035] The present application also provides the use of the above-mentioned conjugated polymer based on fluorine-containing acenaphthene-quinoxaline fused ring units in the preparation of organic solar cell devices.
[0036] The organic solar cell is a bulk heterojunction device. Specifically, the organic solar cell donor material based on the fluorinated acenaphthene-quinoxaline fused ring unit is used as a donor material and is blended with the acceptor material L8-BO as an active layer. Preferably, the organic solar cell donor material based on the fluorinated acenaphthene-quinoxaline fused ring unit and the acceptor L8-BO have a mass ratio of 1:1.5, and the total concentration is 18 mg ml -1 The amount of the additive is 100 wt% relative to the total mass of the donor and the receptor, and the film thickness is 90 to 95 nm.
[0037] Compared with the prior art, the beneficial effects of this application are:
[0038] In the first aspect, the present application achieves a wide optical absorption range, a deep highest occupied molecular orbital (HOMO) energy level and good thermal stability by adjusting the type of electron donating unit in the DA polymer and the length of the alkyl chain on the thiophene bridge based on the organic solar cell donor material containing fluorinated acenaphthene-quinoxaline fused ring units.
[0039] In the second aspect, the donor material of the organic solar cell based on the fluoroacenaphthene-quinoxaline fused ring unit of the present application is easy to obtain, the synthesis is relatively simple, the purification process is simple, the yield is high, and it can be synthesized and prepared on a large scale. The organic solar cell device based on the conjugated polymer containing the fluoroacenaphthene-quinoxaline fused ring unit has a high open circuit voltage, and the optimal device efficiency can reach 12.8%. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 The UV absorption spectra of the solution and film of P1 prepared in the preparation example of this application;
[0041] Figure 2 The UV absorption spectra of the solution and film of P2 prepared in the preparation example of this application;
[0042] Figure 3 The cyclic voltammetry curves of the P1-P2 films prepared in the preparation examples of this application;
[0043] Figure 4 Thermogravimetric analysis diagrams of P1 to P4 prepared in the preparation examples of this application;
[0044] Figure 5 The organic solar cell device structure prepared when P1-P2 prepared in the preparation example of this application is used as a donor material;
[0045] Figure 6 is a current density-voltage performance parameter diagram of the organic solar cell in this application;
[0046] Figure 7 The specific chemical structure diagram of the acceptor material L8-BO used in this application;
[0047] Figure 8 The specific chemical structure diagram of the control group material of this application;
[0048] Fig. 9 This is the hydrogen nuclear magnetic resonance spectrum of the monomer M1 prepared in this application;
[0049] Fig.10 This is the hydrogen nuclear magnetic resonance spectrum of the monomer M2 prepared in this application. DETAILED DESCRIPTION
[0050] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0051] It should be noted that:
[0052] In this application, unless otherwise specified, all the embodiments and preferred implementation methods mentioned herein can be combined with each other to form a new technical solution.
[0053] In the present application, unless otherwise specified, each reaction or operation step can be carried out sequentially or in a sequential manner. Preferably, the reaction method herein is carried out sequentially.
[0054] Unless otherwise specified, the professional and scientific terms used herein are the same as those familiar to those skilled in the art. In addition, any method or material similar or equivalent to the described content may also be applied to the present application.
[0055] The present application provides a conjugated polymer based on a fluorinated acenaphthene-quinoxaline fused ring unit. The structure of the conjugated polymer based on a fluorinated acenaphthene-quinoxaline fused ring unit is shown in the general formula (I):
[0056]
[0057] Wherein, n is the degree of polymerization, which is a natural number selected from 1 to 100, D is the electron donating unit, R 1 and R 2 is independently selected from hydrogen, fluorine, and carbon atoms C 1 ~C 100 Any of a straight chain, branched chain alkyl, alkoxy or sulfanyl group, R 3 It is hydrogen or cyano.
[0058] In the conjugated polymer based on the fluorinated acenaphthene and quinoxaline fused ring unit of the present application, the fluorinated acenaphthene and quinoxaline fused ring unit is used as an electron-withdrawing unit, and a series of conjugated polymer materials are obtained by coupling saturated carbon-carbon bonds with different trimethyltin raw materials through the Stiller reaction using palladium catalysis. Thiophene is used as a π bridge to extend the conjugation length of the polymer main chain, and alkyl chains with different lengths are introduced on thiophene to adjust the aggregation behavior, light absorption range and chemical energy level of the polymer.
[0059] In some preferred embodiments of the present application, the above-mentioned degree of polymerization n is a natural number between 1 and 50.
[0060] In some more preferred embodiments of the present application, the conjugated polymer based on the fluorinated acenaphthene-quinoxaline fused ring unit is selected from any one of the following structural formulas:
[0061]
[0062] On the other hand, the present application provides a method for preparing the above-mentioned conjugated polymer based on fluorinated acenaphthene-quinoxaline fused ring units, comprising the following steps:
[0063] S1. Synthesis of intermediates A1 and A2
[0064] S11. 8,11-dibromo-9,10-difluoroacenaphtho[1,2-b]quinoxaline and tributyl(4-(2-ethylhexyl)thiophen-2-yl)stannane are reacted under the catalysis of tetrakis(triphenylphosphine)palladium to obtain 8,11-bis(4-(2-ethylhexyl)thiophen-2-yl)-9,10-difluoroacenaphtho[1,2-b]quinoxaline A1;
[0065] S12. 8,11-dibromo-9,10-difluoroacenaphtho[1,2-b]quinoxaline and tributyl(4-(2-octyldecyl)thiophen-2-yl)stannane are reacted under the catalysis of tetrakis(triphenylphosphine)palladium to obtain 8,11-bis(4-(2-octyldecyl)thiophen-2-yl)-9,10-difluoroacenaphtho[1,2-b]quinoxaline A2;
[0066] S2. Synthesis of monomers M1 and M2
[0067] S21. A1 in step S11 is reacted with N-bromosuccinimide to obtain 8,11-bis(5-bromo-4-(2-ethylhexyl)thiophen-2-yl)-9,10-difluoroacenaphtho[1,2-b]quinoxaline M1;
[0068] S22. A2 in step S12 is reacted with N-bromosuccinimide to obtain 8,11-bis(5-bromo-4-(2-octyldecyl)thiophen-2-yl)-9,10-difluoroacenaphtho[1,2-b]quinoxaline M2;
[0069] S3. Synthetic polymers P1 to P4
[0070] S31. M1 in step S21 is reacted with (4,8-bis(4-(2-ethylhexyl)-5-fluorothiophen-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) in the presence of tri(dibenzylideneacetone)dipalladium and tri(o-methylphenyl)phosphine using chlorobenzene as solvent, and the polymer P1 is obtained by Soxhlet extraction;
[0071] S32. M1 in step S21 is reacted with (4,8-bis(4-(2-ethylhexyl)-5-chlorothiophene-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) in the presence of tri(dibenzylideneacetone)dipalladium and tri(o-methylphenyl)phosphine using chlorobenzene as solvent, and the polymer P2 is obtained by Soxhlet extraction;
[0072] S33. The M2 in step S22 is reacted with (4,8-bis(4-(2-ethylhexyl)-5-fluorothiophen-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) in the presence of tri(dibenzylideneacetone)dipalladium and tri(o-methylphenyl)phosphine using chlorobenzene as solvent, and the polymer P3 is obtained by Soxhlet extraction;
[0073] S34. The M2 in step S22 is reacted with (4,8-bis(4-(2-ethylhexyl)-5-chlorothiophene-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethyltinane) in the presence of tri(dibenzylideneacetone)dipalladium and tri(o-methylphenyl)phosphine using chlorobenzene as solvent, and the polymer P4 is obtained by Soxhlet extraction.
[0074] In some preferred embodiments, the molar ratio of 8,11-dibromo-9,10-difluoroacenaphtho[1,2-b]quinoxaline, tributyl(4-(2-ethylhexyl)thiophen-2-yl)stannane and tetrakis(triphenylphosphine)palladium catalyst in step S11 is 1:(2.1-2.2):(0.05-0.0.07).
[0075] In some preferred embodiments, the molar ratio of 8,11-dibromo-9,10-difluoroacenaphtho[1,2-b]quinoxaline, tributyl(4-(2-octyldecyl)thiophen-2-yl)stannane and tetrakis(triphenylphosphine)palladium catalyst in step S12 is 1:(2.1-2.2):(0.05-0.0.07).
[0076] In some preferred embodiments, the reaction in step S1 is carried out in an organic solvent under nitrogen protection, the reaction temperature is 120-130° C., and the reaction time is 8-12 h.
[0077] In some preferred embodiments, the molar ratio of A1 to N-bromosuccinimide in step S2 is 1:(2.0-2.1); the molar ratio of A2 to N-bromosuccinimide is 1:(2.0-2.1); the reaction is carried out in an organic solvent and under nitrogen protection, at room temperature in the dark, and the reaction time is 2-4 hours.
[0078] In some preferred embodiments, the molar ratio of M1 and (4,8-bis(4-(2-ethylhexyl)-5-fluorothiophene-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) in step S3 is 1:1; the molar ratio of M1 and (4,8-bis(4-(2-ethylhexyl)-5-chlorothiophene-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) is 1:1; the molar ratio of M2 and (4,8-bis(4-(2-ethylhexyl)-5-fluorothiophene-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) is 1:1. The molar ratio of M2 to (4,8-bis(4-(2-ethylhexyl)-5-chlorothiophen-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethyltinane) is 1:1; the molar ratio of M2 to (4,8-bis(4-(2-ethylhexyl)-5-chlorothiophen-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethyltinane) is 1:1; the reaction is carried out in the dark under nitrogen protection, the mass of tri(dibenzylideneacetone)dipalladium is 6-8 mg, the mass of tri(o-methylphenyl)phosphine is 12-16 mg, and the reaction time is 48 h.
[0079] In some more preferred embodiments, after the reaction described in step S3 is completed, the solution is cooled to room temperature and precipitated with methanol, and then purified by a Soxhlet extractor with methanol, petroleum ether, dichloromethane and chloroform to remove oligomers and residual catalysts, and then the solution is evaporated and concentrated, and precipitated into a methanol solution, and finally the solid is filtered and collected and dried in a vacuum to obtain four conjugated polymers based on fluorinated acenaphthene-quinoxaline fused ring units.
[0080] The present application also provides the use of the above-mentioned conjugated polymer based on fluorine-containing acenaphthene-quinoxaline fused ring units in the preparation of organic solar cell devices.
[0081] Next, the preparation method of the conjugated polymer based on the fluorinated acenaphthene-quinoxaline fused ring unit and the preparation method of the organic solar cell of the present application are described in detail with specific examples.
[0082] Preparation Example Preparation of Conjugated Polymers Based on Fluorinated Acenaphthene-Quinoxaline Condensed Ring Units
[0083] S1. Synthesis of intermediates A1 and A2
[0084] The main synthetic routes of intermediates A1 and A2 are as follows:
[0085]
[0086] S11. Preparation of intermediate A1:
[0087] Tributyl(4-(2-ethylhexyl)thiophen-2-yl)stannane (3.20 g, 6.6 mmol), 8,11-dibromo-9,10-difluoroacenaphtho[1,2-b]quinoxaline (1.34 g, 3.0 mmol), Pd(PPh 3 ) 4 (200 mg, 0.2 mmol) was placed in a pressure bottle reactor and dissolved with 5 mL of DMF, then refluxed under stirring for 12 hours. The organic layer after the crude product was extracted was dried over anhydrous sodium sulfate, filtered, and concentrated by vacuum evaporation. Finally, silica gel column chromatography was used for separation and purification to obtain 8,11-bis(4-(2-ethylhexyl)thiophen-2-yl)-9,10-difluoroacenaphtho[1,2-b]quinoxaline A1.
[0088] S12. Preparation of intermediate A2:
[0089] Tributyl(4-(2-octyldecyl)thiophen-2-yl)stannane (4.31 g, 6.6 mmol), 8,11-dibromo-9,10-difluoroacenaphtho[1,2-b]quinoxaline (1.34 g, 3.0 mmol), Pd(PPh 3 ) 4 (200 mg, 0.2 mmol) was placed in a pressure bottle reactor and dissolved with 5 mL of DMF, then refluxed for 12 hours under stirring. The organic layer after the crude product was extracted was dried over anhydrous sodium sulfate, filtered, and concentrated by vacuum evaporation. Finally, silica gel column chromatography was used for separation and purification to obtain 8,11-bis(4-(2-ethylhexyl)thiophen-2-yl)-9,10-difluoroacenaphtho[1,2-b]quinoxaline A2.
[0090] S2. Synthesis of monomers M1 and M2
[0091] The main synthetic routes of monomers M1 and M2 are as follows:
[0092]
[0093] S21. Preparation of monomer M1:
[0094] A1 (0.68 g, 1 mmol) was dissolved in 15 ml of chloroform, and then NBS (0.36 g, 2.0 mmol) was added in batches and stirred at room temperature for 2 hours. The reaction solution was extracted with dichloromethane, and the organic layer after extraction was dried over anhydrous sodium sulfate. The obtained crude product was further purified by silica gel column chromatography using pure petroleum ether as eluent. Finally, monomer M1 was obtained.
[0095] The monomer M1 was characterized by nuclear magnetic resonance. 1 H NMR (400 MHz, Chloroform-d) δ8.04 (d, J = 6.9 Hz, 2H), 7.96 (d, J = 8.2 Hz, 2H), 7.65 (dd, J = 8.0, 7.1 Hz, 2H), 7.59 (s, 2H), 2.58 (d, J = 7.2 Hz, 4H), 1.74-1.71 (m, 2H), 1.44-1.37 (m, 16H), 0.99-0.93 (m, 12H). The H NMR spectrum of its monomer M1 is shown in Fig. 9 shown.
[0096] Preparation of S22 monomer M2:
[0097] A2 (1.016 g, 1 mmol) was dissolved in 15 ml of chloroform, and then NBS (0.36 g, 2.0 mmol) was added in batches and stirred at room temperature for 2 hours. The reaction solution was extracted with dichloromethane, and the organic layer after extraction was dried over anhydrous sodium sulfate. The obtained crude product was further purified by silica gel column chromatography using pure petroleum ether as eluent. Finally, monomer M2 was obtained.
[0098] The monomer M2 was characterized by nuclear magnetic resonance. 1 H NMR (400 MHz, Chloroform-d) δ8.27 (d, J = 8.0 Hz, 2H), 8.06 (d, J = 8.0 Hz, 2H), 7.77 (dd, J = 8.0, 16.0 Hz, 2H), 7.67 (s, 2H), 2.60 (d, J = 8.0 Hz, 4H), 1.78 (s, 2H), 1.36-1.25 (m, 66H), 0.87-0.83 (m, 12H). The H NMR spectrum of its monomer M2 is shown in Fig.10 shown.
[0099] S3. Synthetic polymers P1 to P4
[0100] S31. Synthesis of polymer P1
[0101] The synthetic route of the DA type conjugated polymer P1 is as follows:
[0102]
[0103] Weigh M1 (83.7 mg, 0.1 mmol) and (4,8-bis(4-(2-ethylhexyl)-5-fluorothiophen-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) (94.3 mg, 0.1 mmol)) into a 15 ml pressure bottle, weigh Pd2 (dba) 3 (6mg) and P(o-tol) 3 (12 mg) was added to a pressure bottle and mixed in 2 ml of chlorobenzene. The reaction mixture was heated to 145 ° C and stirred for 48 hours under a nitrogen atmosphere. After the reaction liquid was cooled to room temperature, the solution was added dropwise to methanol with a glass dropper for precipitation. The solid was collected by filtration through a funnel. The pure crude product was purified by a Soxhlet extractor with methanol, petroleum ether and dichloromethane to remove oligomers and residual catalysts. Finally, the polymer was collected from chloroform. The chloroform solution was then evaporated and concentrated and precipitated into a methanol solution. The solid was collected by filtration and dried in a vacuum to obtain a black polymer solid. The data measured by high temperature GPC are as follows: n = 14.
[0104] S32. Synthesis of polymer P2
[0105] The synthetic route of the DA type conjugated polymer P2 is as follows:
[0106]
[0107] Weigh M1 (83.7 mg, 0.1 mmol) and BDT-Cl (97.3 mg, 0.1 mmol) into a 15 ml pressure bottle.
[0108] Weigh Pd 2 (dba) 3 (6mg) and P(o-tol) 3 (12 mg) was added to a pressure bottle and mixed in 2 ml of chlorobenzene. The reaction mixture was heated to 145 ° C and stirred for 48 hours under a nitrogen atmosphere. After the reaction liquid was cooled to room temperature, the solution was added dropwise to methanol with a glass dropper for precipitation. The solid was collected by filtration through a funnel. The pure crude product was purified by a Soxhlet extractor with methanol, petroleum ether and dichloromethane to remove oligomers and residual catalysts. Finally, the polymer was collected from chloroform. The chloroform solution was then evaporated and concentrated and precipitated into a methanol solution. The solid was collected by filtration and dried in a vacuum to obtain a black polymer solid. The data measured by high temperature GPC are as follows: n = 16.
[0109] S33. Synthesis of polymer P3
[0110] The synthetic route of the DA type conjugated polymer P3 is as follows:
[0111]
[0112] Weigh M2 (117.3 mg, 0.1 mmol) and BDT-F (94.3 mg, 0.1 mmol) into a 15 ml pressure bottle, weigh Pd 2 (dba) 3(6mg) and P(o-tol) 3 (12 mg) was added to a pressure bottle and mixed in 2 ml of chlorobenzene. The reaction mixture was heated to 145 ° C and stirred for 48 hours under a nitrogen atmosphere. After the reaction liquid was cooled to room temperature, the solution was added dropwise to methanol with a glass dropper for precipitation. The solid was collected by filtration through a funnel. The pure crude product was purified by a Soxhlet extractor with methanol, petroleum ether and dichloromethane to remove oligomers and residual catalysts. Finally, the polymer was collected from chloroform. The chloroform solution was then evaporated and concentrated and precipitated into a methanol solution. The solid was collected by filtration and dried in a vacuum to obtain a black polymer solid. The data measured by high temperature GPC are as follows: n = 24.
[0113] S34. Synthesis of polymer P4
[0114] The synthetic route of the DA type conjugated polymer P4 is as follows:
[0115]
[0116] Weigh M2 (117.3 mg, 0.1 mmol) and BDT-Cl (97.3 mg, 0.1 mmol) into a 15 ml pressure bottle, weigh Pd 2 (dba) 3 (6mg) and P(o-tol) 3 (12 mg) was added to a pressure bottle and mixed in 2 ml of chlorobenzene. The reaction mixture was heated to 145 ° C and stirred for 48 hours under a nitrogen atmosphere. After the reaction liquid was cooled to room temperature, the solution was added dropwise to methanol with a glass dropper for precipitation. The solid was collected by filtration through a funnel. The pure crude product was purified by a Soxhlet extractor with methanol, petroleum ether and dichloromethane to remove oligomers and residual catalysts. Finally, the polymer was collected from chloroform. The chloroform solution was then evaporated and concentrated and precipitated into a methanol solution. The solid was collected by filtration and dried in a vacuum to obtain a black polymer solid. The data measured by high temperature GPC are as follows: n = 24.
[0117] Performance Characterization
[0118] The present application provides physical and chemical property test experiments of conjugated polymers P1 to P4 based on fluorinated acenaphthene-quinoxaline fused ring units obtained in the preparation examples, including:
[0119] 1. Preparation Example The UV-visible spectra of the prepared conjugated polymers P1 and P2 based on fluorinated acenaphthene-quinoxaline fused ring units are as follows:
[0120] Weigh 5 mg of the conjugated polymers P1 and P2 containing fluoroacenaphthene-quinoxaline fused ring units prepared in the preparation example and add them to 0.5 ml of chloroform to obtain a 10 mg / ml polymer solution. Use a pipette to take 3 μl of the solution and dilute it 1000 times. Use a Shimadzu 2400 spectrometer to test its absorption in the chloroform solution. For thin film absorption, use a pipette to take 20 μl of the above polymer solution and spin coat it on a quartz plate at a speed of 2000 rpm to obtain a quartz plate carrying a polymer film. Use a Shimadzu 2400 spectrometer to test its thin film absorption test results. See Table 1, and the test spectrum is shown in Figure 1 and Figure 2 .
[0121] Table 1: Absorbance test data of the conjugated polymer materials P1 and P2 solutions and films prepared in the preparation example
[0122]
[0123] pass Figure 1 , Figure 2 As can be seen from Table 1, the organic polymer donor material based on acenaphthene-quinoxaline unit obtained in the present application has a wide absorption range and its solution has a strong absorption range from 300nm to 700nm. It also shows that the organic solar cell donor material based on fluorinated acenaphthene-quinoxaline fused ring unit in the present application achieves a wide optical absorption range by adjusting the type of electron donating unit in the DA polymer and the length of the alkyl chain on the thiophene bridge; at the same time, it is quite matched with the absorption range of commercial non-fullerene acceptor materials, which greatly increases the ability to capture sunlight and is of great help to the device to obtain a high short-circuit current.
[0124] 2. Preparation Example Cyclic voltammetry test of the conjugated polymer based on acenaphthene and quinoxaline units prepared:
[0125] Cyclic voltammetry measurements were performed on a Metrohm Autolab PGSTAT302N electrochemical workstation using a three-electrode system with a glassy carbon electrode as the working electrode, a platinum wire as the counter electrode, and an Ag / Ag as the reference electrode. + The electrode was scanned at 100 mV / s under nitrogen atmosphere. The electrolyte was tetrabutylammonium hexafluorophosphate (Bu 4 NPF 6 ,0.1mol / L), ferrocene (Fc / Fc + ) as internal standard. A 10 mg / ml chloroform solution of polymer P1-P2 was added dropwise onto a platinum carbon electrode to test the energy level using the three-electrode method. Specific data are shown in Table 2, and the spectrum obtained by the test is shown in Figure 3 .
[0126] Table 2: Preparation Example Electrochemical energy level test of the conjugated polymer
[0127]
[0128] The polymers P1~P2 measured by the data all have lower highest occupied orbitals, and the energy level of the material with the highest performance reaches -5.58ev, which means it has a deep highest occupied molecular orbital (HOMO) energy level, which will bring a larger open circuit voltage, which is crucial to improving the performance of organic solar cells.
[0129] 3. Thermogravimetric analysis test of conjugated polymers P1 to P4 based on fluorine-containing acenaphthene and quinoxaline fused ring units obtained in the preparation examples of this application:
[0130] The thermodynamic properties of the material were tested by NETZSCH STA449F5 thermogravimetric analyzer in a nitrogen environment with a heating rate of 10°C / min. The specific data are shown in Table 3 and the spectrum obtained by the test is shown in Figure 4 .
[0131] Table 3: Thermogravimetric analysis of conjugated polymers P1 to P4 based on fluorinated acenaphthene-quinoxaline fused ring units
[0132]
[0133]
[0134] from Figure 4 As shown in Table 3, the 5% thermal weight loss temperatures of the conjugated polymers P1-P4 based on fluorinated acenaphthene-quinoxaline fused ring units are all greater than 400 degrees, indicating that the four compounds have good thermal stability.
[0135] Application Examples
[0136] (1) Pretreatment of ITO glass anode: First, the quartz glass sheet sputtered with ITO was cleaned in an ultrasonic environment. The cleaning solution was conductive glass cleaning solution, deionized water, acetone and ethanol in sequence, and then dried in an oven for 12 hours at a drying temperature of 60°C. Before coating the PEDOT:PSS film, the ITO glass was cleaned with oxygen plasma for 20 minutes, and then the PEDOT:PSS solution was spin-coated at 3000 rpm for 30 seconds and annealed at 150°C for 20 minutes.
[0137] (2) Device preparation: The traditional upright device structure ITO / PEDOT:PSS / active layer / PDIN / Ag was used. The active layer blend solution was spin-coated onto PEDOT:PSS in a nitrogen environment in a glove box at a speed of 2000 rpm for 40 seconds, and then placed on a hot plate for thermal annealing at 80°C for 2 minutes. A methanol solution of PDIN (2 mg / ml) was coated on the static active layer surface, and spin coating was started at an acceleration of 500 rpm / s. The electron transport layer was spin-coated at a speed of 3000 rpm for 30 seconds. In a high vacuum evaporation device, the vacuum was evacuated to 2×10 -4 Pa, a 100 nm silver layer was deposited on the surface of the electron transport layer.
[0138] (3) Device packaging: The fabricated device is sealed in a nitrogen atmosphere glove box, the effective area is covered with glue and a sealing cover and sealed by UV curing.
[0139] The light source was calibrated with a silicon reference cell of an AM 1.5G global solar simulator (Oriel model 91192) with an intensity of 100 mW cm -2 Before the current-voltage (JV) test, a precise area of 4mm 2 The physical mask of the aperture is used to define the device area. For the specific device structure, see Figure 5 The receptor structure used is Figure 7 The corresponding solar cell parameters are shown in Table 4, and the current density-voltage performance parameter diagram of the corresponding organic solar cell is shown in Figure 6 shown.
[0140] Table 4: Test parameters of solar device of P1 and P2 conjugated polymers prepared in the preparation examples, existing similar materials, PT-DTAQx, PF-DTAQx, PC-DTAQx, 2DPBDT-DTOctOxyAQx, PBDT-DTAQx and 2DPBDT-DTAQx as reference group
[0141]
[0142]
[0143] According to Table 4, the open circuit voltage of the conjugated polymers P1 and P2 based on the fluorinated acenaphthene-quinoxaline fused ring unit prepared in the preparation example also exceeds 0.9 V, and the energy conversion efficiency of the optimal material has reached 12.8%, which is comparable to the reported control materials PBDT-DTAQx, PT-DTAQx PF-DTAQX, PC-DTAQx, 2DPBDT-DTAQx and 2DPBDT-DTOctOxyAQx (the corresponding control material structures are shown in Figure 8 ), the performance of the material has been greatly improved, which further enhances the commercialization potential of the organic polymer prepared based on acenaphthene-quinoxaline units in organic solar cells.
[0144] The present application provides a conjugated polymer based on a fluorinated acenaphthene-quinoxaline fused ring unit. The structure of the conjugated polymer based on a fluorinated acenaphthene-quinoxaline fused ring unit is shown in the general formula (I):
[0145]
[0146] Wherein, n is the degree of polymerization, which is a natural number selected from 1 to 100, D is the electron donating unit, R 1 and R 2 is independently selected from hydrogen, fluorine, and carbon atoms C 1 ~C 100 Any of a straight chain, branched chain alkyl, alkoxy or sulfanyl group, R 3 It is hydrogen or cyano.
[0147] In the conjugated polymer based on the fluorinated acenaphthene and quinoxaline fused ring unit of the present application, the fluorinated acenaphthene and quinoxaline fused ring unit is used as the electron-withdrawing unit (A-unit), and the fluorinated or chlorinated unit of benzodithiophene (BDT) is used as the electron-donating unit (D-unit), and four organic solar cell donor materials with DA structure are synthesized. Thiophene is used as a π bridge to extend the conjugated length of the polymer main chain, and alkyl chains with different lengths are introduced on thiophene to adjust the aggregation behavior, light absorption range and chemical energy level of the polymer.
[0148] The polymerization unit (AQx) provided in the present application has few synthetic preparation steps, readily available raw materials, simple synthesis and purification processes, and high yield; the polymer has the advantages of achieving a wide optical absorption range, a deep highest occupied molecular orbital (HOMO) energy level, and good stability.
[0149] Compared with the prior art, this application has the following technical effects:
[0150] In the first aspect, the present application achieves a wide optical absorption range, a deep highest occupied molecular orbital (HOMO) energy level and good thermal stability by adjusting the type of electron donating unit in the DA polymer and the length of the alkyl chain on the thiophene bridge based on the organic solar cell donor material containing fluorinated acenaphthene-quinoxaline fused ring units.
[0151] In the second aspect, the donor material of the organic solar cell based on the fluorinated acenaphthene and quinoxaline fused ring unit of the present application is easy to obtain, the synthesis and purification process is simple, the yield is high, and it can be synthesized and prepared on a large scale. The conjugated polymer organic solar cell device based on the fluorinated acenaphthene and quinoxaline fused ring unit has a high open circuit voltage, and the optimal device efficiency can reach 12.8%.
[0152] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiments or examples are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0153] Although several embodiments of the present application have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the claims and their equivalents.
Claims
1. A conjugated polymer based on a fluorinated acenaphthene-quinoxaline fused ring unit, characterized in that: The structure of the conjugated polymer based on the fluorinated acenaphthene-quinoxaline fused ring unit is shown in the general formula (I): Wherein, n is the degree of polymerization, a natural number selected from 1 to 100, D is an electron donating unit, R1 and R2 are independently selected from hydrogen, fluorine, carbon atoms of C1 to C 100 any one of a straight-chain alkyl group or a branched-chain alkyl group, an alkoxy group or a sulfanyl group, and R3 is hydrogen or a cyano group.
2. The conjugated polymer based on fluorinated acenaphthene-quinoxaline fused ring units according to claim 1, characterized in that: The electron donating unit has any one of the following structural formulas: wherein X is any one independently selected from hydrogen, fluorine, chlorine, bromine and iodine atoms; X1 is any one independently selected from fluorine, chlorine, bromine and iodine atoms; the alkyl chain represented by R is a straight chain or branched chain of 1 to 100 carbon atoms, wherein one or more carbon atoms may be substituted by oxygen atoms, alkenyl groups, alkynyl groups, aryl groups, hydroxyl groups, amino groups, carbonyl groups, carboxyl groups, ester groups, cyano groups and nitro groups, and hydrogen atoms may be substituted by fluorine atoms, oxygen atoms, alkenyl groups, alkynyl groups, aryl groups, hydroxyl groups, amino groups, carbonyl groups, carboxyl groups, ester groups, cyano groups and nitro groups.
3. The conjugated polymer based on fluorinated acenaphthene-quinoxaline fused ring units according to claim 1, characterized in that: The n is a natural number between 1 and 50.
4. The method for preparing a conjugated polymer based on a fluorinated acenaphthene-quinoxaline fused ring unit according to claim 1, characterized in that: The following steps are involved: S1. Synthesis of intermediates A1 and A2 S11. 8,11-dibromo-9,10-difluoroacenaphtho[1,2-b]quinoxaline and tributyl(4-(2-ethylhexyl)thiophen-2-yl)stannane are reacted under the catalysis of tetrakis(triphenylphosphine)palladium to obtain 8,11-bis(4-(2-ethylhexyl)thiophen-2-yl)-9,10-difluoroacenaphtho[1,2-b]quinoxaline A1; S12. 8,11-dibromo-9,10-difluoroacenaphtho[1,2-b]quinoxaline and tributyl(4-(2-octyldecyl)thiophen-2-yl)stannane are reacted under the catalysis of tetrakis(triphenylphosphine)palladium to obtain 8,11-bis(4-(2-octyldecyl)thiophen-2-yl)-9,10-difluoroacenaphtho[1,2-b]quinoxaline A2; S2. Synthesis of monomers M1 and M2 S21. A1 in step S11 is reacted with N-bromosuccinimide to obtain 8,11-bis(5-bromo-4-(2-ethylhexyl)thiophen-2-yl)-9,10-difluoroacenaphtho[1,2-b]quinoxaline M1; S22. A2 in step S12 is reacted with N-bromosuccinimide to obtain 8,11-bis(5-bromo-4-(2-octyldecyl)thiophen-2-yl)-9,10-difluoroacenaphtho[1,2-b]quinoxaline M2; S3. Synthesis of Conjugated Polymers Based on Fluorinated Acenaphthene-Quinoxaline Fused Ring Units S31. M1 in step S21 is reacted with (4,8-bis(4-(2-ethylhexyl)-5-fluorothiophen-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) in the presence of tri(dibenzylideneacetone)dipalladium and tri(o-methylphenyl)phosphine using chlorobenzene as solvent, and the polymer P1 is obtained by Soxhlet extraction; S32. M1 in step S21 is reacted with (4,8-bis(4-(2-ethylhexyl)-5-chlorothiophene-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) in the presence of tri(dibenzylideneacetone)dipalladium and tri(o-methylphenyl)phosphine using chlorobenzene as solvent, and the polymer P2 is obtained by Soxhlet extraction; S33. The M2 in step S22 is reacted with (4,8-bis(4-(2-ethylhexyl)-5-fluorothiophen-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) in the presence of tri(dibenzylideneacetone)dipalladium and tri(o-methylphenyl)phosphine using chlorobenzene as solvent, and the polymer P3 is obtained by Soxhlet extraction; S34. The M2 in step S22 is reacted with (4,8-bis(4-(2-ethylhexyl)-5-chlorothiophene-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethyltinane) in the presence of tri(dibenzylideneacetone)dipalladium and tri(o-methylphenyl)phosphine using chlorobenzene as solvent, and the polymer P4 is obtained by Soxhlet extraction.
5. The method for preparing a conjugated polymer based on a fluorinated acenaphthene-quinoxaline fused ring unit according to claim 4, characterized in that: The molar ratio of 8,11-dibromo-9,10-difluoroacenaphtho[1,2-b]quinoxaline, tributyl(4-(2-ethylhexyl)thiophen-2-yl)stannane and tetrakis(triphenylphosphine)palladium catalyzer in step S11 is 1:(2.1-2.2):(0.05-0.0.07); the molar ratio of 8,11-dibromo-9,10-difluoroacenaphtho[1,2-b]quinoxaline, tributyl(4-(2-octyldecyl)thiophen-2-yl)stannane and tetrakis(triphenylphosphine)palladium catalyzer in step S12 is 1:(2.1-2.2):(0.05-0.0.07).
6. The method for preparing a conjugated polymer based on a fluorinated acenaphthene-quinoxaline fused ring unit according to claim 4, characterized in that: The reaction in step S1 is carried out in an organic solvent under nitrogen protection, the reaction temperature is 120-130° C., and the reaction time is 8-12 h.
7. The method for preparing a conjugated polymer based on a fluorinated acenaphthene-quinoxaline fused ring unit according to claim 4, characterized in that: In step S2, the molar ratio of A1 to N-bromosuccinimide is 1:(2.0-2.1); the molar ratio of A2 to N-bromosuccinimide is 1:(2.0-2.1); the reaction is carried out in an organic solvent and under nitrogen protection, at room temperature in the dark, and the reaction time is 2-4 hours.
8. The method for preparing a conjugated polymer based on a fluorinated acenaphthene-quinoxaline fused ring unit according to claim 4, characterized in that: In step S3, the molar ratio of M1 to (4,8-bis(4-(2-ethylhexyl)-5-fluorothiophene-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) is 1:1; the molar ratio of M1 to (4,8-bis(4-(2-ethylhexyl)-5-chlorothiophene-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) is 1:1; the molar ratio of M2 to (4,8-bis(4-(2-ethylhexyl)-5-fluorothiophene-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) is 1:1 The molar ratio of M2 to (4,8-bis(4-(2-ethylhexyl)-5-chlorothiophene-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) is 1:1; the molar ratio of M2 to (4,8-bis(4-(2-ethylhexyl)-5-chlorothiophene-2-yl)benzo[1,2-b:4,5-b']dithiophene-2,6-diyl)bis(trimethylstannane) is 1:1; the reaction is carried out in the dark under nitrogen protection, the mass of tri(dibenzylideneacetone)dipalladium is 6-8 mg, the mass of tri(o-methylphenyl)phosphine is 12-16 mg, and the reaction time is 48 hours.
9. The method for preparing a conjugated polymer based on a fluorinated acenaphthene-quinoxaline fused ring unit according to claim 4, characterized in that: After the reaction described in step S3 is completed, the mixture is cooled to room temperature and precipitated with methanol, and then purified by a Soxhlet extractor with methanol, petroleum ether, dichloromethane and chloroform to remove oligomers and residual catalysts. The solution is then evaporated and concentrated, and precipitated into a methanol solution. Finally, the solid is collected by filtration and dried in a vacuum to obtain a conjugated polymer based on a fluorinated acenaphthene-quinoxaline fused ring unit.
10. Use of the conjugated polymer based on fluorine-containing acenaphthenequinoxaline fused ring units as claimed in claim 1 in the preparation of organic solar cell devices.
Citation Information
Patent Citations
Conjugated polymer containing naphthalimide substituted quinoxaline and application of conjugated polymer in preparation of organic photovoltaic device
CN117126373A
Organic electroluminescence element, metal complex for organic electroluminescence element, display device, and illumination device
JP2015037138A
Novel polymer, light-emitting device material and light-emitting device using the same
US20010012572A1
Conjugated polymer, insolubilized polymer, organic electroluminescence element material, composition for organic electroluminescence element, polymer production process, organic electroluminescence element, organic el display and organic el lighting
US20110042661A1