Zinc dicarboxylate catalyst, preparation method and application thereof

A high-purity zinc dicarboxylic acid catalyst was prepared by reacting dialkylzinc with a dicarboxylic acid solution under a specific temperature program, which solved the problems of catalyst purity and activity and enabled a highly efficient copolymerization reaction of carbon dioxide and epoxides.

CN119039579AActive Publication Date: 2024-11-29JIANGNAN UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411133800.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-29
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The residual solid zinc source in existing dicarboxylic acid zinc catalysts leads to a decrease in catalyst purity, affecting activity and making it difficult to effectively catalyze the copolymerization reaction of carbon dioxide and epoxides.

Method used

A zinc dicarboxylic acid catalyst was synthesized by precipitation method by reacting a dialkylzinc solution with a dicarboxylic acid solution under a specific temperature program. This controlled particle size and crystallinity, thereby improving the catalyst's purity and activity.

Benefits of technology

The prepared zinc dicarboxylic acid catalyst has high purity and significantly improved activity. It is suitable for the binary copolymerization of carbon dioxide and epoxide, as well as the ternary copolymerization of carbon dioxide, epoxide and cyclic anhydride, exhibiting high catalytic activity and excellent yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039579A_ABST
    Figure CN119039579A_ABST
Patent Text Reader

Abstract

The invention provides a zinc dicarboxylate catalyst as well as a preparation method and application thereof, and belongs to the field of catalysts. The preparation method of the zinc dicarboxylate catalyst comprises the following steps: adding a dialkyl zinc solution into a dicarboxylic acid solution, and preparing the zinc dicarboxylate catalyst through a precipitation method under a specific heating program. The zinc dicarboxylate is a compound with a general formula of Zn-R (COO) 2, wherein R is C1-C8 alkyl. Compared with the prior art, the catalyst obtained by the method has the advantages that on one hand, the purity exceeds 99%, the problem of zinc source residue is avoided, and on the other hand, the catalyst with smaller grain size is prepared by controlling the temperature change. The prepared catalyst is simple in preparation method, is particularly applied to catalysis of binary copolymerization of carbon dioxide and epoxide and ternary copolymerization of carbon dioxide, epoxide and cyclic anhydride, and has the characteristics of high catalyst purity, small particle size and excellent catalytic activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalyst preparation and relates to a dicarboxylate zinc catalyst, a preparation method and application thereof. The catalyst prepared by the method is applied to the polymerization process of carbon dioxide and epoxide, and carbon dioxide, epoxide and cyclic anhydride, and exhibits excellent activity. Background Art

[0002] Over the past century, petroleum-based polymers have replaced traditional natural materials due to their low price and strong durability, completely changing people's lives. However, with the extensive use of these petroleum-based polymers, carbon dioxide emissions are being accelerated, leading to increasingly severe global environmental problems. Therefore, it is becoming a trend to produce polymers with less impact on the environment, such as degradable polyplastics. Among them, carbon dioxide-based polycarbonates prepared with carbon dioxide as a monomer are well-known for their biodegradability and various properties and have attracted widespread attention. Carbon dioxide-based polycarbonates are mainly obtained by the ring-opening copolymerization of carbon dioxide and epoxides. Among them, the most economically valuable one is polypropylene carbonate, which is widely used in medical dressings and packaging films due to its excellent biocompatibility and barrier properties. In addition, the introduction of a third monomer, such as cyclic anhydride, in the copolymerization of carbon dioxide and epoxide can better regulate biodegradability and improve the deficiencies of carbon dioxide-based polycarbonates in thermal and mechanical properties.

[0003] There are many kinds of catalysts currently used in the field of carbon dioxide-based polycarbonate, and it is generally recognized that the catalyst that meets the industrialization route has a dicarboxylic acid zinc catalyst, which has high catalytic efficiency, simple preparation, economical and non-toxic and is easy to separate from the product. M. Ree et al. (Journal of Polymer Science: Part A: Polymer Chemistry, 1999, 37, 1863) added ground zinc oxide to a toluene solution of glutaric acid, reacted at 55 ° C for 4 hours, and the obtained catalyst was used for the alternating copolymerization of carbon dioxide and propylene oxide for 40 hours, and the activity was up to 70g polypropylene carbonate / g catalyst (approximately equivalent to 15.8g polypropylene carbonate / g catalyst / 9 hours). In the post-processing stage of the catalyst, this method only uses acetone as a solvent to wash away the unreacted acid source, and the solid zinc source is retained in the catalyst because it is difficult to remove, resulting in a decrease in catalyst purity and inhibiting the improvement of activity.

[0004] The present invention has found that changing the zinc source to dialkyl zinc can effectively solve the problem of residual solid zinc source, thereby improving the purity of the catalyst. In addition, by adding the dialkyl zinc solution to the dicarboxylic acid solution, the particle size and crystallinity of the catalyst can be controlled by controlling the speed of temperature change, and zinc glutarate crystals with smaller particles and moderate crystallinity can be prepared, thereby further improving the activity of the catalyst. Summary of the invention

[0005] The purpose of the present invention is to provide a zinc dicarboxylate catalyst, a preparation method and application thereof. The catalyst prepared by the method is applied to the polymerization process of carbon dioxide and epoxide, and carbon dioxide, epoxide and cyclic anhydride, and exhibits excellent activity.

[0006] The technical solution of the present invention is:

[0007] A zinc dicarboxylate catalyst, wherein the zinc dicarboxylate catalyst is mainly composed of Zn-R(COO)2, wherein R is a C1-C8 hydrocarbon group, and an XRD spectrum of the zinc dicarboxylate catalyst has diffraction peaks at 2θ angles of 12.90±0.5, 22.80±0.4, and 23.10±0.4, the full width at half maximum is higher than 0.4, the crystallinity is 40-70%, and the specific surface area of ​​the zinc dicarboxylate catalyst is 30-100m 2 / g.

[0008] A preparation method of a zinc dicarboxylate catalyst comprises the following steps: adding a dialkyl zinc solution to a dicarboxylic acid solution, reacting under a specific temperature increase program, synthesizing a crude zinc dicarboxylate catalyst by a precipitation method, and finally washing, filtering and drying to obtain the zinc dicarboxylate catalyst, wherein the purity of the zinc dicarboxylate catalyst is ≥99%. The specific temperature increase program refers to: preparing the dialkyl zinc solution and the dicarboxylic acid solution at a low temperature, the initial temperature of the two after mixing is -5 to 10°C, and the temperature is increased to room temperature at a temperature increase rate of 0.1 to 1°C / min.

[0009] Further, the dialkyl zinc is (C x H 2x+1 )2Zn; the good solvent of the reaction system of dialkyl zinc and dicarboxylic acid R(COOH)2 is C x H 2x+1 OH, C x H 2x+2 , C x H 2x+1 COC x H 2x+1 , C x H 2x+1 OC x H 2x+1 and C x H 2x Oy or a mixture of two or more thereof, wherein R is a 1-C8 hydrocarbon group, x≥1, y≥1.

[0010] Furthermore, the molar ratio of the dialkyl zinc to the dicarboxylic acid is 20:20-22; the mass concentration of the dialkyl zinc solution is 10%-20%; and the mass concentration of the dicarboxylic acid solution is 5%-15%.

[0011] Furthermore, the reaction time under the specific temperature rising program is 1 to 12 hours, and mechanical stirring is performed at a rotation speed of 0 to 3000 rpm during the reaction.

[0012] Furthermore, the dicarboxylic acid is one of succinic acid, glutaric acid, adipic acid, pimelic acid or suberic acid.

[0013] Application of a dicarboxylic acid zinc catalyst prepared by the above preparation method, wherein the dicarboxylic acid zinc catalyst is used for catalyzing the reaction of carbon dioxide and epoxide Binary copolymerization of carbon dioxide, epoxides and cyclic anhydrides A terpolymerization reaction wherein n is 1, 2 or 3; R1 and R2 are epoxy compound substituents; and R3 and R4 are anhydride substituents.

[0014] Furthermore, R1 and R2 are H, CH2Cl, CH2OBn, methyl, benzene ring, cyclohexene, cyclopentene, naphthalene or cyclohexyl, and R1 and R2 are the same or different; R3 and R4 are H, =CH2, benzene ring, cyclohexene or norbornene ring, and R3 and R4 are the same or different.

[0015] Further, the epoxide is propylene oxide, ethylene oxide, cyclohexene oxide, butylene oxide, epichlorohydrin, phenyl glycidyl ether, allyl glycidyl ether, 2-(ethylene oxide ethoxy)tetrahydro-2H-pyran, tetrahydrofuran or styrene oxide; the cyclic anhydride is succinic anhydride, phthalic anhydride, cyclopentane-1,2-dicarboxylic anhydride, cyclopropane-1,2-dicarboxylic anhydride, itaconic anhydride, citraconic anhydride, maleic anhydride or nadic anhydride.

[0016] Furthermore, the copolymerization reaction temperature is 20-120° C., the pressure is 0.1-10 MPa, and the reaction time is 2-100 h.

[0017] The beneficial effects of the present invention are:

[0018] The catalyst prepared by the invention has a simple method and high purity, is applied to catalyze the binary copolymerization reaction of carbon dioxide and epoxide, and the ternary copolymerization reaction of carbon dioxide, epoxide and cyclic anhydride, and has the characteristic of high catalytic activity. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The WXRD spectra of the zinc dicarboxylates prepared in Example 2 and Comparative Examples 1, 2, 4, and 5; wherein ZnGA--10°C is Comparative Example 1, ZnGA-20°C is Comparative Example 2, ZnGA-0.05°C / min is Comparative Example 4, ZnGA-0.20 / min is Example 2, and ZnGA-1.2°C / min is Comparative Example 5;

[0020] Figure 2 Nitrogen adsorption / desorption isotherms of zinc dicarboxylates prepared in Example 2 and Comparative Examples 1, 2, 4, and 5. Among them, ZnGA--10°C is Comparative Example 1, ZnGA-20°C is Comparative Example 2, ZnGA-0.05°C / min is Comparative Example 4, ZnGA-0.20 / min is Example 2, and ZnGA-1.2°C / min is Comparative Example 5. DETAILED DESCRIPTION

[0021] The present invention is described in detail below with reference to the embodiments.

[0022] Embodiment 1:

[0023] Take 20mmol glutaric acid and configure it into a tetrahydrofuran solution with a mass concentration of about 15%, then add it to a 100ml round-bottom flask, set the speed to 1000rpm, slowly add a n-hexane solution with a mass concentration of 20% dissolved with 20mmol diethyl zinc under a -5°C nitrogen environment, and after adding, heat up from -5°C at a rate of 0.1°C / min to room temperature, and react for 12 hours. After the reaction is completed, remove unreacted diethyl zinc and dicarboxylic acid with n-hexane and tetrahydrofuran, respectively, and obtain a dicarboxylic acid zinc catalyst after drying. Add 0.2g of the catalyst in a 100ml autoclave, then add 25ml of propylene oxide, charge with carbon dioxide and heat and pressurize until the pressure in the autoclave reaches 5MPa, the temperature in the autoclave is 60°C, and react for 9 hours. After the reaction is completed, the product discharged from the kettle is added with dichloromethane and stirred to dissolve, and 5% hydrochloric acid is added to remove the residual catalyst, washed with water until neutral, and then methanol is added to precipitate it to wash away impurities such as cyclic carbonate in the polymer, and finally dried to obtain polypropylene carbonate.

[0024] Embodiment 2:

[0025] Take 20mmol glutaric acid and configure it into a tetrahydrofuran solution with a mass concentration of about 15%, then add it to a 100ml round-bottom flask, set the speed to 1000rpm, slowly add a n-hexane solution with a mass concentration of 20% dissolved with 20mmol diethyl zinc under a 0℃ nitrogen environment, and after adding, heat up from 0℃ to room temperature at a rate of 0.2℃ / min, and react for 6 hours. After the reaction is completed, remove unreacted diethyl zinc and dicarboxylic acid with n-hexane and tetrahydrofuran respectively, and obtain a dicarboxylic acid zinc catalyst after drying. Add 0.2g of the catalyst in a 100ml autoclave, then add 25ml of propylene oxide, charge with carbon dioxide and heat and pressurize until the pressure in the autoclave reaches 5MPa, the temperature in the autoclave is 60℃, and react for 9 hours. After the reaction is completed, the product discharged from the kettle is added with dichloromethane and stirred to dissolve, and 5% hydrochloric acid is added to remove the residual catalyst, washed with water until neutral, and then methanol is added to precipitate it to wash away impurities such as cyclic carbonate in the polymer, and finally dried to obtain polypropylene carbonate. Figure 1 The XRD spectrum of the zinc dicarboxylate prepared in Example 2 is shown in FIG. Figure 2 This is the nitrogen adsorption / desorption isotherm of the zinc dicarboxylate prepared in Example 2.

[0026] Embodiment 3:

[0027] Take 20mmol glutaric acid and configure it into a tetrahydrofuran solution with a mass concentration of about 15%, then add it to a 100ml round-bottom flask, set the speed to 1000rpm, slowly add a 20% n-hexane solution dissolved with 20mmol diethyl zinc under a 10°C nitrogen environment, and after adding, heat up from 10°C to room temperature at a rate of 0.9°C / min, and react for 1 hour. After the reaction is completed, remove unreacted diethyl zinc and dicarboxylic acid with n-hexane and tetrahydrofuran, respectively, and obtain a dicarboxylic acid zinc catalyst after drying. Add 0.2g of the catalyst in a 100ml autoclave, then add 25ml of propylene oxide, fill with carbon dioxide and heat and pressurize until the pressure in the autoclave reaches 5MPa, the temperature in the autoclave is 60°C, and react for 9 hours. After the reaction is completed, the product discharged from the kettle is added with dichloromethane and stirred to dissolve, and 5% hydrochloric acid is added to remove the residual catalyst, washed with water until neutral, and then methanol is added to precipitate it to wash away impurities such as cyclic carbonate in the polymer, and finally dried to obtain polypropylene carbonate.

[0028] Embodiment 4:

[0029] Take 22mmol glutaric acid and configure it into a tetrahydrofuran solution with a mass concentration of about 5%, then add it to a 100ml round-bottom flask, set the speed to 1000rpm, slowly add a 20% n-hexane solution dissolved with 20mmol diisopropyl zinc under a 5°C nitrogen environment, and after adding, heat up from 5°C to room temperature at a rate of 0.5°C / min, and react for 4 hours. After the reaction is completed, remove the unreacted diisopropyl zinc and dicarboxylic acid with n-hexane and tetrahydrofuran, respectively, and obtain a dicarboxylic acid zinc catalyst after drying. Add 0.2g of the catalyst in a 100ml autoclave, then add 25ml of propylene oxide, fill with carbon dioxide and heat and pressurize until the pressure in the autoclave reaches 5MPa, the temperature in the autoclave is 60°C, and react for 9 hours. After the reaction is completed, the product discharged from the kettle is added with dichloromethane and stirred to dissolve, and 5% hydrochloric acid is added to remove the residual catalyst, washed with water until neutral, and then methanol is added to precipitate it to wash away impurities such as cyclic carbonate in the polymer, and finally dried to obtain polypropylene carbonate.

[0030] Embodiment 5:

[0031] Take 20mmol adipic acid and configure it into a tetrahydrofuran solution with a mass concentration of about 5%, then add it to a 100ml round-bottom flask, set the speed to 1000rpm, slowly add a 15% n-hexane solution with 20mmol diethyl zinc dissolved in a 0℃ nitrogen environment, and after adding, heat up from 0℃ to room temperature at a rate of 0.2℃ / min, and react for 6 hours. After the reaction is completed, remove the unreacted diethyl zinc and dicarboxylic acid with n-hexane and tetrahydrofuran respectively, and obtain a dicarboxylic acid zinc catalyst after drying. Add 0.2g of the catalyst into a 100ml autoclave, then add 25ml of propylene oxide, fill with carbon dioxide and heat and pressurize until the pressure in the autoclave reaches 5MPa, the temperature in the autoclave is 60℃, and react for 9 hours. After the reaction is completed, the product discharged from the kettle is added with dichloromethane and stirred to dissolve, and 5% hydrochloric acid is added to remove the residual catalyst, washed with water until neutral, and then methanol is added to precipitate it to wash away impurities such as cyclic carbonate in the polymer, and finally dried to obtain polypropylene carbonate.

[0032] Embodiment 6:

[0033] Take 20mmol glutaric acid and configure it into a tetrahydrofuran solution with a mass concentration of about 5%, then add it to a 100ml round-bottom flask, set the speed to 1000rpm, slowly add a n-hexane solution with a mass concentration of 15% dissolved with 20mmol diethyl zinc under a 0℃ nitrogen environment, and after adding, heat up from 0℃ to room temperature at a rate of 0.2℃ / min, and react for 6 hours. After the reaction is completed, remove unreacted diethyl zinc and dicarboxylic acid with n-hexane and tetrahydrofuran respectively, and obtain a dicarboxylic acid zinc catalyst after drying. Add 0.2g of the catalyst in a 100ml autoclave, then add 25ml of ethylene oxide, charge with carbon dioxide and heat and pressurize until the pressure in the autoclave reaches 1MPa, the temperature in the autoclave is 40℃, and react for 9 hours. After the reaction is completed, the product discharged from the kettle is added with dichloromethane and stirred to dissolve, and 5% hydrochloric acid is added to remove the residual catalyst, washed with water until neutral, and then methanol is added to precipitate it to wash away impurities such as cyclic carbonate in the polymer, and finally dried to obtain polyvinyl carbonate.

[0034] Embodiment 7:

[0035] Take 20mmol glutaric acid and configure it into a tetrahydrofuran solution with a mass concentration of about 5%, then add it to a 100ml round-bottom flask, set the speed to 1000rpm, slowly add a n-hexane solution with a mass concentration of 15% dissolved with 20mmol diethyl zinc under a 0°C nitrogen environment, and after adding, heat up from 0°C to room temperature at a rate of 0.2°C / min, and react for 6 hours. After the reaction is completed, remove unreacted diethyl zinc and dicarboxylic acid with n-hexane and tetrahydrofuran, and obtain a dicarboxylic acid zinc catalyst after drying. Add 0.2g of the catalyst in a 100ml autoclave, then add 20ml of propylene oxide and 2.8g of maleic anhydride, charge with carbon dioxide and heat and pressurize, so that the pressure in the autoclave reaches 5MPa, the temperature in the autoclave is 60°C, and react for 9 hours. After the reaction is completed, the product discharged from the kettle is added into dichloromethane and stirred to dissolve, and 5% hydrochloric acid is added to remove the residual catalyst and acid anhydride, and then methanol is added to make it precipitate to wash away impurities such as cyclic carbonate in the polymer, and finally dried to obtain a terpolymer.

[0036] Embodiment 8:

[0037] Take 20mmol glutaric acid and configure it into a tetrahydrofuran solution with a mass concentration of about 5%, then add it to a 100ml round-bottom flask, set the speed to 1000rpm, slowly add a n-hexane solution with a mass concentration of 15% dissolved with 20mmol diethyl zinc under a 5℃ nitrogen environment, and after adding, heat up from 5℃ to room temperature at a rate of 0.5℃ / min, and react for 4 hours. After the reaction is completed, remove unreacted diethyl zinc and dicarboxylic acid with n-hexane and tetrahydrofuran, respectively, and obtain a dicarboxylic acid zinc catalyst after drying. Add 0.2g of the catalyst in a 100ml autoclave, then add 20ml of propylene oxide and 2.8g of itaconic anhydride, charge with carbon dioxide and heat and pressurize, so that the pressure in the autoclave reaches 5MPa, the temperature in the autoclave is 70℃, and react for 9 hours. After the reaction is completed, the product discharged from the kettle is added into dichloromethane and stirred to dissolve, and 5% hydrochloric acid is added to remove the residual catalyst and acid anhydride, and then methanol is added to make it precipitate to wash away impurities such as cyclic carbonate in the polymer, and finally dried to obtain a terpolymer.

[0038] Comparative Example 1 (compared with Example 2):

[0039] Take 20mmol of glutaric acid and prepare a tetrahydrofuran solution with a mass concentration of about 15%, then add it to a 100ml round-bottom flask, set the rotation speed to 1000rpm, add a 20% n-hexane solution containing 20mmol of diethyl zinc under a nitrogen environment at -10℃, and react at -10℃ for 6h after adding. After the reaction is completed, remove the unreacted diethyl zinc and dicarboxylic acid with n-hexane and tetrahydrofuran respectively, and obtain the dicarboxylic acid zinc catalyst after drying. Add 0.2g of the catalyst to a 100ml autoclave, then add 25ml of propylene oxide, fill with carbon dioxide and heat and pressurize so that the pressure in the autoclave reaches 5MPa, the temperature in the autoclave is 60℃, and react for 9 hours. After the reaction is completed, add dichloromethane to the product discharged from the autoclave and stir to dissolve, add 5% hydrochloric acid to remove the residual catalyst, wash with water until neutral, then add methanol to precipitate it, wash away impurities such as cyclic carbonate in the polymer, and finally dry to obtain polypropylene carbonate. Attached Figure 1 The XRD spectrum of the zinc dicarboxylate prepared in Comparative Example 1 is shown in FIG. Figure 2 This is the nitrogen adsorption / desorption isotherm curve of the zinc dicarboxylate prepared in Comparative Example 1.

[0040] Comparative Example 2 (compared with Example 2):

[0041] Take 20mmol of glutaric acid and prepare a tetrahydrofuran solution with a mass concentration of about 15%, then add it to a 100ml round-bottom flask, set the rotation speed to 1000rpm, add a 20% n-hexane solution containing 20mmol of diethyl zinc under a 20℃ nitrogen environment, and react at 20℃ for 6h after adding. After the reaction is completed, remove the unreacted diethyl zinc and dicarboxylic acid with n-hexane and tetrahydrofuran respectively, and obtain the dicarboxylic acid zinc catalyst after drying. Add 0.2g of the catalyst to a 100ml autoclave, then add 25ml of propylene oxide, fill with carbon dioxide and heat and pressurize so that the pressure in the autoclave reaches 5MPa, the temperature in the autoclave is 60℃, and react for 9 hours. After the reaction is completed, add dichloromethane to the product discharged from the autoclave and stir to dissolve, add 5% hydrochloric acid to remove the residual catalyst, wash with water until neutral, then add methanol to precipitate it, wash away impurities such as cyclic carbonate in the polymer, and finally dry to obtain polypropylene carbonate. Attached Figure 1 The XRD spectrum of the zinc dicarboxylate prepared in Comparative Example 2 is shown in FIG. Figure 2 This is the nitrogen adsorption / desorption isotherm curve of the zinc dicarboxylate prepared in Comparative Example 2.

[0042] Comparative Example 3 (compared with Example 2):

[0043] Take 20mmol glutaric acid and configure it into a tetrahydrofuran solution with a mass concentration of about 15%, then add it to a 100ml round-bottom flask, set the speed to 1000rpm, add a n-hexane solution with a mass concentration of 20% dissolved in 20mmol diethyl zinc under a 0℃ nitrogen environment, and react at 0℃ for 6h after adding. After the reaction is completed, remove the unreacted diethyl zinc and dicarboxylic acid with n-hexane and tetrahydrofuran respectively, and obtain a dicarboxylic acid zinc catalyst after drying. Add 0.2g of the catalyst in a 100ml autoclave, then add 25ml of propylene oxide, fill with carbon dioxide and heat and pressurize so that the pressure in the autoclave reaches 5MPa, the temperature in the autoclave is 60℃, and react for 9 hours. After the reaction is completed, add dichloromethane to the product discharged from the autoclave, stir and dissolve, add 5% hydrochloric acid, remove the residual catalyst, wash with water to neutrality, then add methanol to precipitate it, wash away impurities such as cyclic carbonate in the polymer, and finally obtain polypropylene carbonate after drying.

[0044] Comparative Example 4 (compared with Example 2):

[0045] Take 20mmol glutaric acid and configure it into a tetrahydrofuran solution with a mass concentration of about 15%, then add it to a 100ml round-bottom flask, set the speed to 1000rpm, add a 20% n-hexane solution with a mass concentration of 20mmol diethyl zinc under a 0℃ nitrogen environment, and after adding, heat from 0℃ to room temperature at a rate of 0.05℃ / min. After 6h of reaction, remove the unreacted diethyl zinc and dicarboxylic acid with n-hexane and tetrahydrofuran respectively, and obtain the dicarboxylic acid zinc catalyst after drying. Add 0.2g of the catalyst to a 100ml autoclave, then add 25ml of propylene oxide, fill with carbon dioxide and heat and pressurize so that the pressure in the autoclave reaches 5MPa, the temperature in the autoclave is 60℃, and react for 9 hours. After the reaction is completed, add dichloromethane to the product discharged from the autoclave, stir and dissolve, add 5% hydrochloric acid, remove the residual catalyst, wash with water to neutrality, then add methanol to precipitate it, wash away impurities such as cyclic carbonate in the polymer, and finally dry to obtain polypropylene carbonate. Attached Figure 1 The XRD spectrum of the zinc dicarboxylate prepared in Comparative Example 4 is shown in FIG. Figure 2 This is the nitrogen adsorption / desorption isotherm curve of the zinc dicarboxylate prepared in Comparative Example 4.

[0046] Comparative Example 5 (compared with Example 2):

[0047] Take 20mmol glutaric acid and configure it into a tetrahydrofuran solution with a mass concentration of about 15%, then add it to a 100ml round-bottom flask, set the speed to 1000rpm, add a 20% n-hexane solution with a mass concentration of 20mmol diethyl zinc under a 0℃ nitrogen environment, and after adding, heat from 0℃ to room temperature at a rate of 1.2℃ / min. After 6h of reaction, remove the unreacted diethyl zinc and dicarboxylic acid with n-hexane and tetrahydrofuran respectively, and obtain the dicarboxylic acid zinc catalyst after drying. Add 0.2g of the catalyst to a 100ml autoclave, then add 25ml of propylene oxide, fill with carbon dioxide and heat and pressurize to make the pressure in the autoclave reach 5MPa, the temperature in the autoclave is 60℃, and react for 9 hours. After the reaction is completed, add dichloromethane to the product discharged from the autoclave, stir and dissolve, add 5% hydrochloric acid, remove the residual catalyst, wash with water to neutrality, then add methanol to precipitate it, wash away impurities such as cyclic carbonate in the polymer, and finally dry to obtain polypropylene carbonate. Attached Figure 1 For comparison of the XRD spectra of the zinc dicarboxylate prepared in 5, Figure 2 This is the nitrogen adsorption / desorption isotherm curve of the zinc dicarboxylate prepared in Comparative Example 5.

[0048] Comparative Example 6 (compared with Example 2):

[0049] Take 20mmol glutaric acid to make a tetrahydrofuran solution with a mass concentration of about 15%, then add it to a 100ml round-bottom flask, set the speed to 1000rpm, add 20mmol zinc acetate dissolved in 20% acetone solution under 0℃ nitrogen environment, and after adding, heat from 0℃ to room temperature at a rate of 0.2℃ / min. After 6h reaction, remove the unreacted zinc acetate and dicarboxylic acid with acetone and tetrahydrofuran respectively, and obtain the dicarboxylic acid zinc catalyst after drying. Add 0.2g of the catalyst to a 100ml autoclave, then add 25ml of propylene oxide, fill with carbon dioxide and heat and pressurize so that the pressure in the autoclave reaches 5MPa, the temperature in the autoclave is 60℃, and react for 9 hours. After the reaction is completed, add dichloromethane to the product discharged from the autoclave, stir and dissolve, add 5% hydrochloric acid, remove the residual catalyst, wash with water to neutrality, then add methanol to precipitate it, wash away impurities such as cyclic carbonate in the polymer, and finally dry to obtain polypropylene carbonate.

[0050] Comparative Example 7 (compared with Example 2):

[0051] Take 20mmol 2,2-dimethylglutaric acid and prepare a tetrahydrofuran solution with a mass concentration of about 15%, then add it to a 100ml round-bottom flask, set the rotation speed to 1000rpm, add a 20% n-hexane solution with 20mmol diethyl zinc dissolved in a 0℃ nitrogen environment, and after adding, increase the temperature from 0℃ to room temperature at a rate of 0.2℃ / min. After 6h of reaction, remove the unreacted diethyl zinc and dicarboxylic acid with n-hexane and tetrahydrofuran respectively, and obtain a dicarboxylic acid zinc catalyst after drying. Add 0.2g of the catalyst to a 100ml autoclave, then add 25ml of propylene oxide, fill with carbon dioxide and heat and pressurize until the pressure in the autoclave reaches 5MPa, the temperature in the autoclave is 60℃, and react for 9 hours. After the reaction is completed, the product discharged from the kettle is added with dichloromethane and stirred to dissolve, and 5% hydrochloric acid is added to remove the residual catalyst, washed with water until neutral, and then methanol is added to precipitate it to wash away impurities such as cyclic carbonate in the polymer, and finally dried to obtain polypropylene carbonate.

[0052] Comparative Example 8:

[0053] Take 98mmol of zinc oxide, 100mmol of glutaric acid, and 250ml of toluene, add them to a 500ml round-bottom flask, react for 24h under vigorous stirring at 55℃, wash with tetrahydrofuran several times after the reaction is completed, and finally dry to obtain zinc glutarate catalyst. Add 0.2g of catalyst to a 100ml autoclave, then add 25ml of propylene oxide, fill with carbon dioxide and heat and pressurize to make the pressure in the autoclave reach 5MPa, the temperature in the autoclave is 60℃, and react for 9 hours. After the reaction is completed, add dichloromethane to the product discharged from the autoclave, stir and dissolve, add 5% hydrochloric acid, remove the residual catalyst, wash with water to neutrality, then add methanol to precipitate it, wash away impurities such as cyclic carbonate in the polymer, and finally dry to obtain polypropylene carbonate.

[0054] Comparative Example 9:

[0055] Take 98mmol of zinc oxide, 100mmol of adipic acid, and 250ml of toluene, add them to a 500ml round-bottom flask, react for 24h at 55℃ with vigorous stirring, wash with tetrahydrofuran several times after the reaction, dry and finally obtain zinc adipate catalyst. Add 0.2g of catalyst to a 100ml autoclave, then add 25ml of propylene oxide, fill with carbon dioxide and heat and pressurize to make the pressure in the autoclave reach 5MPa, the temperature in the autoclave is 60℃, and react for 9 hours. After the reaction is completed, add dichloromethane to the product discharged from the autoclave, stir and dissolve, add 5% hydrochloric acid, remove the residual catalyst, wash with water until neutral, then add methanol to precipitate it, wash away impurities such as cyclic carbonate in the polymer, and finally dry to obtain polypropylene carbonate.

[0056] Comparative Example 10:

[0057] Take 98mmol of zinc oxide, 100mmol of glutaric acid, and 250ml of toluene, add them to a 500ml round-bottom flask, react for 24h under vigorous stirring at 55℃, wash with tetrahydrofuran several times after the reaction is completed, and finally dry to obtain zinc glutarate catalyst. Add 0.2g of catalyst to a 100ml autoclave, then add 25ml of ethylene oxide, fill with carbon dioxide and heat and pressurize to make the pressure in the autoclave reach 1MPa, the temperature in the autoclave is 40℃, and react for 9 hours. After the reaction is completed, add dichloromethane to the product discharged from the autoclave, stir and dissolve, add 5% hydrochloric acid, remove the residual catalyst, wash with water until neutral, then add methanol to precipitate it, wash away impurities such as cyclic carbonate in the polymer, and finally dry to obtain polyvinyl carbonate.

[0058] Comparative Example 11:

[0059] Take 98mmol of zinc oxide, 100mmol of glutaric acid, and 250ml of toluene, add them to a 500ml round-bottom flask, react for 24h under vigorous stirring at 55℃, wash with tetrahydrofuran several times after the reaction, dry and finally obtain zinc glutarate catalyst. Add 0.2g of the catalyst to a 100ml autoclave, then add 20ml of propylene oxide and 2.8g of maleic anhydride respectively, fill with carbon dioxide and heat and pressurize to make the pressure in the autoclave reach 5MPa, the temperature in the autoclave is 60℃, and react for 9 hours. After the reaction is completed, add dichloromethane to the product discharged from the autoclave, stir and dissolve, add 5% hydrochloric acid to remove the residual catalyst and anhydride, then add methanol to make it precipitate, wash away impurities such as cyclic carbonate in the polymer, and finally dry to obtain a terpolymer.

[0060] Comparative Example 12:

[0061] Take 98mmol of zinc oxide, 100mmol of glutaric acid, and 250ml of toluene, add them to a 500ml round-bottom flask, react for 24h under vigorous stirring at 55℃, wash with tetrahydrofuran several times after the reaction, dry and finally obtain zinc glutarate catalyst. Add 0.2g of the catalyst to a 100ml autoclave, then add 20ml of propylene oxide and 2.8g of itaconic anhydride respectively, fill with carbon dioxide and heat and pressurize to make the pressure in the autoclave reach 5MPa, the temperature in the autoclave is 70℃, and react for 9 hours. After the reaction is completed, add dichloromethane to the product discharged from the autoclave, stir and dissolve, add 5% hydrochloric acid to remove the residual catalyst and anhydride, then add methanol to make it precipitate, wash away impurities such as cyclic carbonate in the polymer, and finally dry to obtain a terpolymer.

[0062] The catalysts in the above examples were used to catalyze the preparation of binary copolymers and ternary copolymers. The polymerization results are shown in Table 1:

[0063] Table 1

[0064]

[0065]

[0066] The WXRD spectra, nitrogen adsorption / desorption isotherms and purities of the zinc dicarboxylates prepared in Example 2 and Comparative Examples 1, 2, 4 and 5 were analyzed. The results are shown in Table 2:

[0067] Table 2

[0068]

[0069] As shown in Table 1, in combination with the data of Comparative Examples 8-12 and Examples 1-8, the dicarboxylic acid zinc catalyst prepared by the present invention is applied to catalyze the binary copolymerization of carbon dioxide and epoxide, and the ternary copolymerization of carbon dioxide, epoxide and cyclic anhydride, and its activity is significantly higher than that of the dicarboxylic acid zinc prepared by the traditional method. Compared with Comparative Examples 1, 2 and 3, the initial reaction temperature is too low or too high, which will significantly reduce the activity of the catalyst. In combination with the data of Example 1 and Comparative Examples 4 and 5, a slower or faster heating rate will also reduce the activity of the catalyst.

[0070] As can be seen from Table 1, the catalyst of the present invention is used to catalyze the binary copolymerization reaction of carbon dioxide and epoxide, and the ternary copolymerization reaction of carbon dioxide, epoxide and cyclic anhydride. The preparation method is simple, the purity is high, and the yield has obvious advantages compared with those reported in previous literature and patents.

[0071] It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in the various embodiments of the present invention described above can be combined with each other as long as they do not conflict with each other. In addition, the above are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present invention.

Claims

1. A zinc dicarboxylate catalyst, characterized in that The zinc dicarboxylate catalyst is mainly composed of Zn-R(COO)2, R is a C1-C8 hydrocarbon group, and the XRD spectrum of the zinc dicarboxylate catalyst has diffraction peaks at 2θ angles of 12.90±0.5, 22.80±0.4, and 23.10±0.4, the full width at half maximum is higher than 0.4, the crystallinity is 40-70%, and the specific surface area of ​​the zinc dicarboxylate catalyst is 30-100m 2 / g.

2. The method for preparing a zinc dicarboxylate catalyst according to claim 1, characterized in that: The following steps are involved: A dialkyl zinc solution is added to a dicarboxylic acid solution, and the reaction is carried out under a specific temperature increase program, a crude dicarboxylic acid zinc catalyst is synthesized by a precipitation method, and finally the dicarboxylic acid zinc catalyst is obtained by washing, filtering and drying, and the purity of the dicarboxylic acid zinc catalyst is ≥99%; the specific temperature increase program refers to: the dialkyl zinc solution and the dicarboxylic acid solution are prepared at a low temperature, the initial temperature of the two after mixing is -5 to 10°C, and the temperature is increased to room temperature at a heating rate of 0.1 to 1°C / min.

3. The method for preparing a dicarboxylic acid zinc catalyst according to claim 2, wherein: Dialkylzinc is (C x H 2x+1 )2Zn; the good solvent of the reaction system of dialkyl zinc and dicarboxylic acid R(COOH)2 is C x H 2x+1 OH, C x H 2x+2 , C x H 2x+ 1COC x H 2x+1 , C x H 2x+1 OC x H 2x+1 and C x H 2x O y or a mixture of two or more thereof, wherein R is a 1-C8 hydrocarbon group, x≥1, y≥1.

4. The method for preparing a dicarboxylic acid zinc catalyst according to claim 2, wherein: The molar ratio of the dialkyl zinc to the dicarboxylic acid is 20:20-22; the mass concentration of the dialkyl zinc solution is 10%-20%; and the mass concentration of the dicarboxylic acid solution is 5%-15%.

5. A method for preparing a dicarboxylic acid zinc catalyst according to claim 2, characterized in that: The reaction time for the reaction under a specific temperature rising program is 1 to 12 hours, and mechanical stirring is performed at a rotation speed of 0 to 3000 rpm during the reaction.

6. A zinc dicarboxylate catalyst according to claim 3, characterized in that: The dicarboxylic acid is one of succinic acid, glutaric acid, adipic acid, pimelic acid or suberic acid.

7. Use of a zinc dicarboxylate catalyst according to claim 1, or a zinc dicarboxylate catalyst prepared by any one of the preparation methods of claims 2 to 6, characterized in that: The dicarboxylic acid zinc catalyst is used for catalyzing the reaction of carbon dioxide and epoxide Binary copolymerization of carbon dioxide, epoxides and cyclic anhydrides A terpolymerization reaction wherein n is 1, 2 or 3; R1 and R2 are epoxy compound substituents; and R3 and R4 are anhydride substituents.

8. The use of a dicarboxylic acid zinc catalyst according to claim 7, characterized in that: R1 and R2 are H, CH2Cl, CH2OBn, methyl, benzene ring, cyclohexene, cyclopentene, naphthalene or cyclohexyl, and R1 and R2 are the same or different; R3 and R4 are H, =CH2, benzene ring, cyclohexene or norbornene ring, and R3 and R4 are the same or different.

9. The use of a dicarboxylic acid zinc catalyst according to claim 7, characterized in that: The epoxide is propylene oxide, ethylene oxide, cyclohexene oxide, butylene oxide, epichlorohydrin, phenyl glycidyl ether, allyl glycidyl ether, 2-(ethylene oxide ethoxy)tetrahydro-2H-pyran, tetrahydrofuran or styrene oxide; the cyclic anhydride is succinic anhydride, phthalic anhydride, cyclopentane-1,2-dicarboxylic anhydride, cyclopropane-1,2-dicarboxylic anhydride, itaconic anhydride, citraconic anhydride, maleic anhydride or nadic anhydride.

10. Use of a dicarboxylate zinc catalyst according to claim 7, 8 or 9, characterized in that: The copolymerization reaction temperature is 20-120°C, the pressure is 0.1-10MPa, and the reaction time is 2-100h.

Citation Information

Patent Citations

  • Method for producing zinc dicarboxylate

    CN103781817A

  • Method for preparing zinc dicarboxylate catalyst, modified zinc dicarboxylate catalyst and carbon dioxide-epoxide copolymer

    CN105418907A

  • Organic zinc catalyst, method for manufacturing same, and method for preparing polyalkylene carbonate resin using organic zinc catalyst

    CN106457212A

  • Organic zinc catalyst and preparation method thereof

    US20160222159A1