Preparation method of fully-biodegradable high-toughness lignin / PBAT (poly (butylene adipate-co-terephthalate)) film
By introducing toughening additives such as cellulose acetate and glycerol into the lignin/PBAT film, combined with oleic amide and other components, and processing through a mixer and a twin-screw extruder, the lignin/PBAT film in the prior art was solved. The problem of insufficient material toughness has achieved the preparation and cost reduction of high-tough films, and promoted green and sustainable development.
Patent Information
- Application Number
- CN202411214400.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-31
- Publication Date
- 2024-11-29
AI Technical Summary
When the existing methods improve the toughness of lignin/PBAT film materials, there is insufficient cleaning, non-renewable, and non-degradable reagents. The modification steps are complicated and the process is long, and the preparation of lignin doping additives is complicated and expensive, which limits the Large-scale application of lignin/PBAT enhanced toughening film materials.
The mixture of cellulose acetate and glycerol is used as a toughening additive, combined with oleic amide, polyethylene glycol and other ingredients, and is thoroughly mixed and granulated through a mixer and a twin screw extruder, followed by hot pressing to prepare High toughness lignin/PBAT film.
It significantly improves the elongation of lignin/PBAT films for breaking, expands its application range, and reduces material production costs, reduces dependence on oil resources and carbon emissions, and promotes green and sustainable development.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the field of plastics, and in particular to a method for preparing a fully biodegradable, high-toughness lignin / PBAT film. Background Art
[0002] Synthetic plastics are playing an increasingly significant role in our production activities and daily life. At present, with the continuous improvement of people's consumption level, the consumption of plastic products is gradually increasing. However, the production and use of petroleum-based materials including polyethylene, polyvinyl chloride, styrene and polyethylene terephthalate will produce a large amount of greenhouse gases.
[0003] Polybutylene terephthalate / adipate (PBAT) is a fully biodegradable polyester that can be decomposed by enzymes in microorganisms and plants and animals in the natural environment, and eventually degraded into water and carbon dioxide, with sustainable development characteristics. This material not only has good thermal stability and excellent processing performance, but also has good ductility and high elongation at break. Therefore, it is widely used in packaging materials, agricultural films, disposable tableware and other fields. However, PBAT is expensive, and low-cost, biodegradable fillers are often added to reduce production costs.
[0004] Lignin is the most abundant aromatic polymer in nature, mainly composed of phenylpropane structural units, with the characteristics of wide sources, low cost, strong rigidity and biodegradability. In many studies and patents, lignin is added to PBAT as a filler to reduce the production cost of PBAT and achieve enhancement at the same time. However, lignin has a three-dimensional rigid structure, and the addition of lignin will cause the elongation at break, i.e., the toughness of the PBAT film material, to decrease significantly. At present, the method for improving the toughness of lignin / PBAT film materials lies in modifying lignin, adding additives, and the like. For example, Chinese patents CN114474449 B and CN202110778500.8 both report methods for preparing biodegradable plastics by using modified lignin composite PBAT, and the enhancement and toughening of lignin / PBAT film materials are achieved by regulating and improving the hydrophobicity of lignin. CN113402857B reports the use of metal coordination additives to composite lignin and then dope micro or nano cellulose to achieve enhancement and toughening.
[0005] The existing methods have the problems that the modification reagents are not clean enough, are non-renewable, and non-degradable, and the modification steps are cumbersome and the process is long. In addition, the preparation of lignin doping additives is complicated and expensive, and the metal coordination compounds are non-biodegradable, which limits the large-scale application of lignin / PBAT reinforced and toughened film materials. Summary of the invention
[0006] In order to solve the shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a method for preparing a fully biodegradable, high-toughness lignin / PBAT film. The method has the characteristics of simple operation, clean and pollution-free, and easy to scale up and promote.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] Step (1): Drying a certain amount of PBAT masterbatch and lignin respectively;
[0009] Step (2): adding the dried PBAT, lignin and toughening agent, as well as lubricant, plasticizer, antioxidant and antistatic agent into an internal mixer, and mixing them thoroughly to obtain a mixed material;
[0010] Step (3): Extruding the obtained mixture through a twin-screw extruder to obtain lignin-PBAT composite plastic pellets;
[0011] Step (4): hot-pressing the lignin-PBAT composite plastic particles at a certain temperature to obtain a lignin-PBAT film.
[0012] Specifically, the lignin in step (1) is selected from DCL lignin, alkali lignin, kraft lignin, lignin sulfonate, etc., and has a particle size of 100 to 600 meshes; preferably, the particle size is 200 to 400 meshes.
[0013] Specifically, the drying process in step (1) is: drying temperature is 22-42°C, drying time is 1h-3h, and vacuum degree is 0-5000Pa (absolute pressure); preferably, the drying temperature is 26-36°C, the drying time is 2h-2.5h, and the vacuum degree is 500-3000Pa (absolute pressure); more preferably, the drying temperature is 29-32°C, the drying time is 2.3h, and the vacuum degree is 1000-2000Pa (absolute pressure).
[0014] Specifically, in step (2), the toughening aid is a mixture of cellulose acetate (CA) and glycerol, preferably the weight ratio of CA:glycerol is 10:1 to 1:1, and the cellulose acetate is preferably cellulose acetate produced by MacLean Company, with an acetyl content of 16.8 to 39.5wt%, a hydroxyl content of 4.0wt%, and a molecular weight of 30,000 to 60,000.
[0015] Specifically, in step (2), the lubricant is selected from one of oleic acid amide, erucic acid amide, bis-stearic acid amide, and calcium stearate; the plasticizer is selected from one of polyethylene glycol (PEG), Joncryl ADR-4370S, triethyl citrate (TEC), phthalic anhydride (PA), 2,2-(1,3-phenylene)bis(2-oxazoline) (BOZ), and 1,6-hexanediol diglycidyl ether, or a mixture of two or more thereof; the antioxidant is selected from one of butylated hydroxytoluene, butylated p-diphenol, diisodecyl phosphite, pentaerythritol bisphosphite, and 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate pentaerythritol ester, or a mixture of two or more thereof; the antistatic agent is selected from one of stearic acid trimethylammonium chloride, stearic acid trimethylammonium chloride, ethoxylated aliphatic alkylamine, and a polyethylene carrier.
[0016] Specifically, in step (2), the mixing temperature of the internal mixer is 130 to 180° C., preferably 150 to 160° C., the rotation speed is 60 r / min, and the mixing time is 15 to 30 min.
[0017] Specifically, in step (3), the extrusion temperature of the twin-screw extruder is 130-180°C, preferably 140-170°C, and more preferably 155-165°C.
[0018] Specifically, in step (4), the temperature of the upper and lower plates of the hot press is 140-180° C.; preferably 150-160° C., the hot pressing time is 10-30 min, and the pressure is 1-8 MPa.
[0019] Specifically, in the toughening method of the lignin / PBAT film, the amount of each raw material is as follows by weight:
[0020]
[0021] Preferably, in the toughening method of the lignin / PBAT film, the amount of each raw material is as follows in parts by weight:
[0022]
[0023] The present invention adopts the above technical solution, which has the following technical effects compared with the prior art:
[0024] (1) The present invention introduces a toughening agent on the basis of preparing the lignin-PBAT film, thereby enhancing the toughness of the film and greatly improving the elongation at break of the composite film. This improvement expands the application range of the film, which is not only suitable for agricultural films, such as ground films and vegetable greenhouse films, but also for a variety of film materials such as degradable packaging bags and injection molded sheets.
[0025] (2) The present invention utilizes lignin powder made from abundant biomass resources in nature and combines it with PBAT to form a new membrane material, thereby forming a new type of membrane material. This combination not only reduces the production cost of the material, but also enhances its competitiveness in the market.
[0026] (3) Compared with traditional petroleum-based film materials, the lignin-PBAT biodegradable film material prepared by the present invention not only helps to reduce white pollution, but also reduces dependence on petroleum resources and carbon emissions in the production process. It can promote the green and sustainable development of the economy. DETAILED DESCRIPTION
[0027] The present invention is further described below by means of specific examples to provide a better understanding of the present invention.
[0028] Example 1
[0029] (I) The proportions of the raw materials used are as follows:
[0030]
[0031] (ii) The specific preparation method comprises the following steps:
[0032] (1) Dry a certain amount of PBAT masterbatch and lignin powder (200 mesh) at 25°C and 0-5000Pa for 2.5h;
[0033] (2) Add dried PBAT, lignin powder, erucamide, PEG2000, butylated hydroxytoluene, and Yamaichi plasticizer antistatic agent SY-193 into an internal mixer, control the material temperature of the internal mixer to 150-160°C, the mixing time to 20 minutes, and the speed to 60 r / min;
[0034] (3) pelletizing the completely mixed materials through a twin-screw extruder, while adjusting the extrusion temperature to 155-165° C. to produce lignin-PBAT composite plastic particles;
[0035] (4) The lignin-PBAT composite plastic particles were hot-pressed, the upper and lower plate temperatures of the hot press were controlled to be 155°C, the hot-pressing time was 20 min, the pre-pressing stage pressure was set to 1.2-2.0 MPa, and the pressurizing stage pressure was set to 5-8 MPa, to obtain a toughened lignin-PBAT film with a thickness of 0.1-0.3 mm.
[0036] Example 2
[0037] (I) The proportions of the raw materials used are as follows:
[0038]
[0039] (ii) For the specific preparation method, refer to Example 1.
[0040] Example 3
[0041] (I) The proportions of the raw materials used are as follows:
[0042]
[0043] (ii) For the specific preparation method, refer to Example 1.
[0044] Example 4
[0045] (I) The proportions of the raw materials used are as follows:
[0046]
[0047] (ii) The specific preparation method comprises the following steps:
[0048] (1) Dry a certain amount of PBAT masterbatch and lignin powder (200 mesh) at 25°C and 0-5000Pa for 2.5h;
[0049] (2) Add dried PBAT, lignin powder, mixed toughening agent, erucic acid amide, PEG2000, butylated hydroxytoluene, and Yamaichi plasticizing antistatic agent SY-193 into an internal mixer, control the material temperature of the internal mixer to 155-160°C, the mixing time to 30 minutes, and the speed to 60 r / min;
[0050] (3) pelletizing the completely mixed materials through a twin-screw extruder, while adjusting the extrusion temperature to 155-165° C. to produce lignin-PBAT composite plastic particles;
[0051] (4) The lignin-PBAT composite plastic particles were hot-pressed, the upper and lower plate temperatures of the hot press were controlled to be 160°C, the hot pressing time was 30 min, the pre-pressing stage pressure was set to 1.2-2.0 MPa, and the pressurizing stage pressure was set to 5-8 MPa, to obtain a toughened lignin-PBAT film with a thickness of 0.1-0.3 mm.
[0052] Example 5
[0053] (I) The proportions of the raw materials used are as follows:
[0054]
[0055]
[0056] (ii) For specific preparation method, refer to Example 4.
[0057] Example 6
[0058] (I) The proportions of the raw materials used are as follows:
[0059]
[0060] (ii) For specific preparation method, refer to Example 4.
[0061] Comparative Example 1
[0062] (I) The proportions of the raw materials used are as follows:
[0063]
[0064] (ii) The specific preparation method comprises the following steps:
[0065] (1) Dry a certain amount of PBAT masterbatch and lignin powder (200 mesh) at 25°C and 0-5000Pa for 2.5h;
[0066] (2) Add dried PBAT, lignin powder, mixed toughening agent, erucic acid amide, PEG2000, butylated hydroxytoluene, and Yamaichi plasticizing antistatic agent SY-193 into an internal mixer, control the material temperature of the internal mixer to 150-160°C, the mixing time to 15 minutes, and the speed to 60 r / min;
[0067] (3) pelletizing the completely mixed materials through a twin-screw extruder, while adjusting the extrusion temperature to 155-165° C. to produce lignin-PBAT composite plastic particles;
[0068] (4) The lignin-PBAT composite plastic particles were hot-pressed, the upper and lower plate temperatures of the hot press were controlled to be 155°C, the hot pressing time was 15 min, the pre-pressing stage pressure was set to 1.2-2.0 MPa, and the pressurizing stage pressure was set to 5-8 MPa, to obtain a toughened lignin-PBAT film with a thickness of 0.1-0.3 mm.
[0069] This comparative example is a lignin-PBAT film without adding a toughening agent under a lignin loading of 10 parts.
[0070] Comparative Example 2
[0071] (I) The proportions of the raw materials used are as follows:
[0072]
[0073] (ii) The specific preparation method comprises the following steps:
[0074] (1) Dry a certain amount of PBAT masterbatch and lignin powder (200 mesh) at 25°C and 0-5000Pa for 2.5h;
[0075] (2) Add dried PBAT, lignin powder, mixed toughening agent, erucic acid amide, PEG2000, butylated hydroxytoluene, and Yamaichi plasticizing antistatic agent SY-193 into an internal mixer, control the material temperature of the internal mixer to 155-160°C, the mixing time to 20 minutes, and the speed to 60 r / min;
[0076] (3) pelletizing the completely mixed materials through a twin-screw extruder, while adjusting the extrusion temperature to 155-165° C. to produce lignin-PBAT composite plastic particles;
[0077] (4) The lignin-PBAT composite plastic particles are hot-pressed, the upper and lower plate temperatures of the hot press are controlled to be 160°C, the hot pressing time is 20 min, the pre-pressing stage pressure is set to 1.2-2.0 MPa, and the pressurizing stage pressure is set to 5-8 MPa, to obtain a toughened lignin-PBAT film with a thickness of 0.1-0.3 mm.
[0078] This comparative example is a lignin-PBAT film without adding a toughening agent under a lignin loading of 20 parts.
[0079] Performance Testing
[0080] The modulus, tensile strength and elongation at break of the above-mentioned Examples 1 to 6 and Comparative Examples 1 and 2 were measured using a microcomputer-controlled electronic universal testing machine (E43.104, manufactured by Mester Industrial Systems (China) Co., Ltd.) in accordance with GBT 1040.3-2006. The specific test results are shown in Table 1:
[0081] Table 1
[0082] Modulus / MPa Elongation at break / % Tensile strength / MPa Example 1 57 217 8.9 Example 2 63 300 9.2 Example 3 52 449 10.1 Example 4 51 142 7.8 Example 5 60 189 8.1 Example 6 58 289 8.7 Comparative Example 1 73 72 8 Comparative Example 2 93 30 6.9
[0083] By analyzing the test data in Table 1, we can observe that compared with the original lignin-PBAT film (Comparative Examples 1 and 2), the toughened lignin-PBAT film (Examples 1 to 6) has achieved significant improvement in mechanical properties.
[0084] Specifically, Comparative Example 1 is a lignin-PBAT film without a toughening agent at a lignin loading of 10 parts, and Examples 1, 2, and 3 are films with a toughening agent added at a lignin loading of 10 parts. The results show that the elongation at break of Examples 1 to 3 is increased by 201%, 317%, and 524% respectively relative to Comparative Example 1.
[0085] Comparative Example 2 is a lignin-PBAT film without a toughening agent at a lignin loading of 20 parts, and Examples 4, 5, and 6 are films with a toughening agent added at a lignin loading of 20 parts. The results show that the elongation at break of Examples 4 to 6 is increased by 373%, 530%, and 863% respectively relative to Comparative Example 2, indicating that its toughness is significantly enhanced. In addition, as the amount of toughening agent added increases, the toughening effect of the film becomes more and more significant. These comparative results fully demonstrate the advantages of the present invention.
[0086] Among them, in Examples 1, 2 and 3, 6, 11 and 16 parts by weight of toughening aid were added successively at a lignin loading of 10 parts by weight. The results show that as the content of toughening aid increases, the toughening effect on the film becomes more significant. In Examples 4, 5 and 6, 6, 11 and 16 parts by weight of toughening aid were added successively at a lignin loading of 20 parts by weight. Combined with the above examples, it is shown that as the lignin loading increases, the toughening effect of the toughening aid on the film is also very significant.
Claims
1. A method for preparing a fully biodegradable, high-toughness lignin / PBAT film, characterized in that: It includes the following steps: Step (1): Drying the PBAT masterbatch and lignin separately; Step (2): adding dried PBAT, lignin and toughening agent, as well as lubricant, plasticizer, antioxidant and antistatic agent into an internal mixer, and mixing them thoroughly to obtain a mixed material; Step (3): Extruding the obtained mixture through a twin-screw extruder to obtain lignin-PBAT composite plastic pellets; Step (4): hot-pressing the lignin-PBAT composite plastic particles to obtain a lignin-PBAT film.
2. The method according to claim 1, characterized in that The lignin in step (1) is selected from DCL lignin, alkali lignin, kraft lignin, and lignin sulfonate, and preferably has a particle size of 100 to 600 meshes; more preferably, has a particle size of 200 to 400 meshes.
3. The method according to claim 1, characterized in that The drying process in step (1) is: drying temperature is 22-42°C, drying time is 1 h-3 h, and vacuum degree is 0-5000 Pa (absolute pressure); preferably, the drying temperature is 26-36°C, the drying time is 2 h-2.5 h, and the vacuum degree is 500-3000 Pa (absolute pressure); more preferably, the drying temperature is 29-32°C, the drying time is 2.3 h, and the vacuum degree is 1000-2000 Pa (absolute pressure).
4. The method according to claim 1, characterized in that In the step (2), the toughening agent is a mixture of cellulose acetate CA and glycerol, preferably the weight ratio of CA to glycerol is 10:1 to 1:1; Preferably, the cellulose acetate is cellulose acetate produced by McLean Company, with an acetyl content of 16.8-39.5wt%, a hydroxyl content of 4.0wt%, and a molecular weight of 30,000-60,000.
5. The method according to claim 1, characterized in that In the step (2), the lubricant is selected from one of oleic acid amide, erucic acid amide, bis-stearic acid amide, and calcium stearate; the plasticizer is selected from one of polyethylene glycol PEG, Joncryl ADR-4370S, triethyl citrate TEC, phthalic anhydride PA, 2,2-(1,3-phenylene)bis(2-oxazoline) BOZ, 1,6-hexanediol diglycidyl ether, or a mixture of two or more thereof; the antioxidant is selected from one of butylated hydroxytoluene, butylated p-diphenol, diisodecyl phosphite, pentaerythritol bisphosphite, and 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate pentaerythritol ester, or a mixture of two or more thereof; the antistatic agent is selected from one of stearic acid trimethylammonium chloride, stearic acid trimethylammonium chloride, ethoxylated aliphatic alkylamine, and polyethylene carrier.
6. The method according to claim 1, characterized in that In the step (2), the mixing temperature of the internal mixer is 130 to 180° C., preferably 150 to 160° C., the rotation speed is 60 r / min, and the mixing time is 15 to 30 min.
7. The method according to claim 1, characterized in that In the step (3), the extrusion temperature of the twin-screw extruder is 130 to 180°C, preferably 140 to 170°C, and more preferably 155 to 165°C.
8. The method according to claim 1, characterized in that In the step (4), the temperature of the upper and lower plates of the hot press is 140 to 180° C., preferably 150 to 160° C., the hot pressing time is 10 to 30 minutes, and the pressure is 1 to 8 MPa.
9. The method according to claim 1, characterized in that The proportions of each raw material by weight are as follows: PBAT 50~100 copies 5-30 parts of lignin Toughening agent 1-20 parts Lubricant 0.3~1 part Plasticizer 0.5~4 parts Antioxidant 0.05~0.4 parts Antistatic agent 0.2-0.8 parts; Preferably, the dosage of each raw material is as follows by weight: PBAT 65~85 parts 10-20 parts of lignin Toughening agent 6-16 parts Lubricant 0.5~0.8 parts 1-3 parts of plasticizer Antioxidant 0.1-0.3 parts Antistatic agent 0.4-0.6 parts.
10. A fully biodegradable, high-toughness lignin / PBAT film obtained by the method according to any one of claims 1 to 9.
Citation Information
Cited By
Torreya grandis shell-based bioplastic and preparation method thereof
CN120399289A