High-reflection coating for surface of lightweight porous material and preparation method of high-reflection coating

By using a composite structural coating composed of oxide filler and Al (H2PO4)3 on the surface of lightweight porous materials, the problem of coating the high-reflective coating on the surface of lightweight porous materials is solved, and efficient cooling and heat insulation effect is achieved. High temperature stability.

CN119039808APending Publication Date: 2024-11-29AEROSPACE INST OF ADVANCED MATERIALS & PROCESSING TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411183030.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art is difficult to effectively apply a highly reflective coating on the surface of lightweight porous materials, resulting in poor cooling and heat insulation effects.

Method used

Spherical powder is prepared by spray drying using a composite structure coating composed of oxide fillers (such as Zr, Ti, Zn, Al, Y, Hf, Ta, Ce oxide) and base material (Al(H2PO4)3). , and apply it to the surface of lightweight porous materials in a brushed manner, combining a gradient curing process to ensure the stability and bond strength of the coating.

Benefits of technology

It realizes efficient cooling and heat insulation on the surface of lightweight porous materials, the reflectivity of the coating is greater than 90% in the 1-2.5μm band, and remains stable at high temperatures, significantly improving the thermal insulation ability of the porous materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039808A_ABST
    Figure CN119039808A_ABST
Patent Text Reader

Abstract

The invention discloses a high-reflection coating for the surface of a light porous material and a preparation method of the high-reflection coating, and belongs to the field of new materials. The high-reflection coating is of a multiphase structure and is composed of oxide filler and a base material Al (H2PO4) 3. According to the invention, oxide filler particles are dispersed into an Al (H2PO4) 3 solution, and a gradient curing mode is adopted, so that a firmly-bonded high-reflection coating can be formed on the surface of a lightweight porous material. The high-reflectivity coating has excellent bonding strength, the filler is prepared through spray drying and is of a spherical structure formed by bonding fine particles, and the reflectivity of the coating can be improved to the maximum extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a high-reflection coating suitable for the surface of a lightweight porous material and a preparation method thereof, and belongs to the field of new materials. Background Art

[0002] The storage of flammable and explosive materials is crucial to production safety. At present, storage buildings usually use reflective coatings for cooling and heat insulation. This coating can play a certain role in cooling and heat insulation, but currently this coating is often applied to the surface of metal or dense non-metallic materials. With the application of porous insulation materials such as aerogels, insulation tiles, and rigid porous foams, it has become necessary to apply reflective coatings on the surface of porous materials. How to prepare high-reflective coatings for the surface of lightweight porous materials has become an urgent problem to be solved. Summary of the invention

[0003] The purpose of the present invention is to provide a high-reflective coating suitable for the surface of lightweight porous materials and a preparation method thereof. The reflective coating is a complex phase structure composed of an oxide filler and a base material, and can be coated on the surface of a lightweight porous material by brushing to play a role in cooling, heat insulation and protection.

[0004] The technical solution adopted by the present invention to achieve the above-mentioned purpose is as follows:

[0005] In the first aspect, the present invention provides a high reflective coating suitable for the surface of a lightweight porous material, wherein the coating raw materials include an oxide filler and a base material, wherein the oxide filler is MO x , M is one of Zr, Ti, Zn, Al, Y, Hf, Ta, and Ce, the base material is Al(H2PO4)3, and the oxide filler and the base material constitute a complex phase structure.

[0006] Furthermore, the oxide filler is a spherical powder formed by bonding submicron particles.

[0007] Furthermore, the submicron particles have a particle size of 0.5 to 1 μm.

[0008] Furthermore, the thickness of the reflective coating is 0.5-3 mm.

[0009] Furthermore, the oxide filler accounts for 30% to 50% of the total mass of the oxide filler and the base material.

[0010] In a second aspect, the present invention further provides a method for preparing a high-reflective coating suitable for the surface of a lightweight porous material, comprising the following steps:

[0011] (1) Select oxide MO x, M is one of Zr, Ti, Zn, Al, Y, Hf, Ta, and Ce, which is added to deionized water to form a suspension, and an organic solvent is added to the suspension;

[0012] (2) using the above suspension as a raw material to prepare spherical powder by spray drying;

[0013] (3) sieving the obtained spherical powder to obtain a spherical powder with a diameter of 10 to 30 μm;

[0014] (4) adding spherical powder of 10 to 30 μm in a mass fraction of 30% to 50% into Al(H2PO4)3 solution to obtain a glue solution, and uniformly dispersing the glue solution by magnetic stirring;

[0015] (5) Accurately weigh the required volume of glue according to the coating area through a measuring cylinder, and use a brush to dip a small amount of glue, evenly apply it on the lightweight porous material substrate, and let it stand at room temperature. The humidity should be controlled at 40% to 50% during standing;

[0016] (6) The coating after standing is placed in an oven for curing, and then naturally cooled to room temperature to obtain a highly reflective coating.

[0017] Furthermore, in step (1), the particle size of the oxide is 0.5-1 μm, the solid content of the suspension is 45%-55%, and the organic solvent is 0.5% by mass of PVA (polyvinyl alcohol), PAA (polyacrylic acid) or HEC (hydroxyethyl methyl cellulose).

[0018] Furthermore, when preparing the spherical powder in step (2), the upper port temperature of the spray granulation equipment is 250-280° C., the lower port temperature is 100-110° C., the spray head speed is 37-43 rpm, and the feed pump speed is 30-40 rpm.

[0019] Furthermore, the density of the Al(H2PO4)3 solution in step (4) is 1.4-1.5 g / cm 3 , stirring speed is 250-350rpm, and stirring time is 1-3h.

[0020] Furthermore, in step (5), the lightweight porous material matrix is ​​an inorganic non-metallic porous material matrix, such as porous foam, aerogel, thermal insulation tile, etc., and is left to stand at room temperature for 24 to 48 hours.

[0021] Furthermore, in step (6), the curing process is as follows: heating to 70-90°C at 3°C / min, keeping warm for 1-2h, heating to 100-120°C at 5°C / min, keeping warm for 2-4h, heating to 140-160°C at 5°C / min, keeping warm for 2-4h, heating to 170-190°C at 5°C / min, keeping warm for 12-24h.

[0022] The beneficial effects achieved by the present invention are as follows:

[0023] 1. The present invention uses Al(H2PO4)3 as an adhesive and adopts a gradient curing method, which can be firmly bonded on the surface of porous materials and has excellent bonding strength.

[0024] 2. The oxide filler MO used in the present invention x (M is Zr, Ti, Zn, Al, Y, Hf, Ta) the powder has a spherical structure and the largest specific surface area. The interface area of ​​the filler is increased, which helps to improve the overall infrared reflectivity of the coating. At the same time, the spherical filler is made of a large number of fine powders bonded together, and the number of interfaces inside the filler is large, which further improves the reflectivity of the coating. The average reflectivity of the coating in the 1-2.5μm band is greater than 90%, which solves the problem of low reflectivity of the coating.

[0025] 3. The present invention proposes a MO x +Al(H2PO4)3 multiphase gradient structure coating, MO x It has good high temperature stability and compatibility with Al(H2PO4)3, and the two-phase structure is stable without phase change, which enables the coating to be used at higher temperatures. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a photo of the physical morphology of the high-reflective coating prepared in Example 1;

[0027] Figure 2 is a reflectivity curve diagram of the high reflective coating prepared in Example 1;

[0028] Figure 3 This is a photo of the physical morphology of the high-reflective coating prepared in Example 2;

[0029] Figure 4 is a reflectivity curve diagram of the high reflective coating prepared in Example 2;

[0030] Figure 5 This is a photo of the physical morphology of the high-reflective coating prepared in Example 3;

[0031] Figure 6 This is a reflectivity curve of the high-reflection coating prepared in Example 3. DETAILED DESCRIPTION

[0032] In order to make the various technical features and advantages or technical effects in the above technical solutions of the present invention more obvious and easy to understand, they are described in detail below with reference to the accompanying drawings.

[0033] Example 1

[0034] A method for preparing a high-reflective coating suitable for the surface of a lightweight porous material comprises the following steps:

[0035] (1) TiO2 with a particle size of 0.5 μm was selected and added to deionized water to prepare a suspension. The solid content of the suspension was 45%, and PVA with a mass fraction of 0.5% was added to the suspension.

[0036] (2) The suspension was used as a raw material to prepare a spherical powder by spray drying. During spray drying, the upper port temperature was 250° C., the lower port temperature was 100° C., the spray head speed was 37 rpm, and the feed pump speed was 30 rpm.

[0037] (3) The obtained spherical TiO2 powder is sieved to obtain spherical powder with a diameter of 10 to 30 μm.

[0038] (4) adding the obtained TiO2 spherical powder into the Al(H2PO4)3 solution at a mass fraction of 30%, and uniformly dispersing the obtained colloid by magnetic stirring at a stirring speed of 250 rpm for 1 h;

[0039] (5) Accurately weigh the required volume of glue according to the coating area through a measuring cylinder, and use a brush to dip a small amount of glue, evenly apply it on the porous material substrate, and let it stand at room temperature for 24 hours. The humidity should be controlled at 40% during the standing time;

[0040] (6) The coating after standing is placed in an oven for curing. The curing process is as follows: heating to 80°C at 3°C / min, keeping warm for 1 hour, heating to 120°C at 5°C / min, keeping warm for 2 hours, heating to 150°C at 5°C / min, keeping warm for 2 hours, heating to 170°C at 5°C / min, keeping warm for 12 hours, and then cooling to room temperature with the oven;

[0041] (7) Measure the coating thickness using a micrometer and repeat steps (5) and (6) until the thickness reaches 3 mm.

[0042] After testing, the bonding strength of the coating is 2.936MPa. After coating, the thermal insulation capacity of the porous material is increased by 18.7%. Example 2

[0043] A method for preparing a high-reflective coating suitable for the surface of a lightweight porous material comprises the following steps:

[0044] (1) ZrO2 with a particle size of 1 μm was selected and added to deionized water to prepare a suspension with a solid content of 55%. PVA (polyvinyl alcohol) with a mass fraction of 0.5% was added to the suspension.

[0045] (2) The suspension was used as a raw material to prepare a spherical powder by spray drying. During spray drying, the upper port temperature was 280° C., the lower port temperature was 110° C., the spray head speed was 43 rpm, and the feed pump speed was 40 rpm.

[0046] (3) The obtained spherical ZrO2 powder is sieved to obtain spherical powder with a diameter of 10 to 30 μm.

[0047] (4) adding the obtained ZrO2 spherical powder into the Al(H2PO4)3 solution at a mass fraction of 50%, and uniformly dispersing the obtained colloid by magnetic stirring at a stirring speed of 350 rpm for 3 h;

[0048] (5) Accurately weigh the required volume of glue according to the coating area through a measuring cylinder, and use a brush to dip a small amount of glue, evenly apply it on the porous material substrate, and let it stand at room temperature for 36 hours. The humidity should be controlled at 45% during the standing time;

[0049] (6) The coating after standing was placed in an oven for curing. The curing process was as follows: heating to 70°C at 3°C / min, keeping the temperature for 2h, heating to 110°C at 5°C / min, keeping the temperature for 3h, heating to 140°C at 5°C / min, keeping the temperature for 4h, heating to 190°C at 5°C / min, keeping the temperature for 18h, and then cooling to room temperature with the oven;

[0050] (7) Measure the coating thickness using a micrometer and repeat steps (5) and (6) until the thickness reaches 0.5 mm.

[0051] After testing, the bonding strength of the coating was found to be 3.842MPa, and after application of the coating, the thermal insulation capacity of the porous material was increased by 21.4%.

[0052] Example 3

[0053] A method for preparing a high-reflective coating suitable for the surface of a lightweight porous material comprises the following steps:

[0054] (1) TiO2 with a particle size of 0.7 μm was selected and added to deionized water to prepare a suspension with a solid content of 50%. PVA with a mass fraction of 0.5% was added to the suspension.

[0055] (2) The suspension was used as a raw material to prepare a spherical powder by spray drying. During spray drying, the upper port temperature was 270° C., the lower port temperature was 105° C., the spray head speed was 40 rpm, and the feed pump speed was 35 rpm.

[0056] (3) The obtained spherical TiO2 powder is sieved to obtain spherical powder with a diameter of 10 to 30 μm.

[0057] (4) adding the obtained TiO2 spherical powder into the Al(H2PO4)3 solution at a mass fraction of 40%, and uniformly dispersing the obtained colloid by magnetic stirring at a stirring speed of 300 rpm for 3 h;

[0058] (5) Accurately weigh the required volume of glue according to the coating area through a measuring cylinder, and use a brush to dip a small amount of glue, evenly apply it on the porous material substrate, and let it stand at room temperature for 48 hours. The humidity should be controlled at 50% during the standing time;

[0059] (6) The coating after standing is placed in an oven for curing. The curing process is as follows: heating to 90°C at 3°C / min, keeping warm for 1.5 hours, heating to 100°C at 5°C / min, keeping warm for 4 hours, heating to 160°C at 5°C / min, keeping warm for 3 hours, heating to 180°C at 5°C / min, keeping warm for 24 hours, and then cooling to room temperature with the oven;

[0060] (7) Measure the coating thickness using a micrometer and repeat steps (5) and (6) until the thickness reaches 2 mm.

[0061] After testing, the bonding strength of the coating was found to be 3.574MPa, and after application of the coating, the thermal insulation capacity of the porous material was increased by 19.6%.

[0062] Although the present invention has been disclosed as above by way of embodiments, it is not intended to limit the present invention. Appropriate modifications or equivalent substitutions of the technical solutions of the present invention made by ordinary technicians in the field should all be included in the protection scope of the present invention. The protection scope of the present invention shall be based on what is defined in the claims.

Claims

1. A high reflective coating suitable for the surface of a lightweight porous material, characterized in that: The coating materials include oxide filler and base material, wherein the oxide filler is MO x , M is one of Zr, Ti, Zn, Al, Y, Hf, Ta, and Ce, the base material is Al(H2PO4)3, and the oxide filler and the base material constitute a complex phase structure.

2. The high reflective coating according to claim 1, characterized in that The oxide filler is a spherical powder formed by bonding particles with a particle size of 0.5 to 1 μm.

3. The high reflective coating according to claim 1 or 2, characterized in that: The oxide filler accounts for 30% to 50% of the total mass of the oxide filler and the base material.

4. A method for preparing a high-reflective coating suitable for the surface of a lightweight porous material, characterized in that: The following steps are involved: (1) Select oxide MO x , M is one of Zr, Ti, Zn, Al, Y, Hf, Ta, and Ce, which is added to deionized water to form a suspension, and an organic solvent is added to the suspension; (2) using the above suspension as a raw material to prepare spherical powder by spray drying; (3) sieving the obtained spherical powder to obtain a spherical powder with a diameter of 10 to 30 μm; (4) adding spherical powder of 10 to 30 μm in a mass fraction of 30% to 50% into Al(H2PO4)3 solution to obtain a glue solution, and uniformly dispersing the glue solution by magnetic stirring; (5) Accurately weigh the required volume of glue according to the coating area through a measuring cylinder, and use a brush to dip a small amount of glue, evenly apply it on the lightweight porous material substrate, and let it stand at room temperature. The humidity should be controlled at 40% to 50% during standing; (6) The coating after standing is placed in an oven for curing, and then naturally cooled to room temperature to obtain a highly reflective coating.

5. The preparation method according to claim 4, characterized in that: In step (1), the particle size of the oxide is 0.5 to 1 μm, and the solid content of the suspension is 45% to 55%.

6. The preparation method according to claim 4, characterized in that: The organic solvent is 0.5% by mass of PVA, PAA or HEC.

7. The preparation method according to claim 4, characterized in that: When preparing spherical powder in step (2), the upper port temperature of the spray granulation equipment is 250-280° C., the lower port temperature is 100-110° C., the rotation speed of the spray head is 37-43 rpm, and the feed pump speed is 30-40 rpm.

8. The preparation method according to claim 4, characterized in that: The density of the Al(H2PO4)3 solution in step (4) is 1.4-1.5 g / cm 3 , stirring speed is 250-350rpm, and stirring time is 1-3h.

9. The preparation method according to claim 4, characterized in that: In step (5), the mixture is allowed to stand at room temperature for 24 to 48 hours.

10. The preparation method according to claim 4, characterized in that: The curing process in step (6) is as follows: heating to 70-90°C at 3°C / min, keeping warm for 1-2h, heating to 100-120°C at 5°C / min, keeping warm for 2-4h, heating to 140-160°C at 5°C / min, keeping warm for 2-4h, heating to 170-190°C at 5°C / min, keeping warm for 12-24h.

Citation Information

Patent Citations

  • Reflective substrate for light-emitting element and method for producing same

    CN103477458A

  • Reflecting coating material for solar energy double-sided power generation double-glass assembly

    CN108455954A

  • High-temperature-resistant insulation coating and preparation method thereof

    CN109897400A

  • Preparation method of lanthanum zirconate spherical powder for thermal spraying

    CN111153434A

  • Hydrophobic moisture-proof layer of wave-transparent material and preparation method of hydrophobic moisture-proof layer

    CN115625099A