Urea-formaldehyde resin modified adhesive and application thereof in production of all-elm super-strong high-moisture-proof shaving board

Through the combination technology of cross-linking melamine and urea formaldehyde resin in modified urea formaldehyde resin adhesive and carbon nanotubes absorb formaldehyde, the problems of high formaldehyde content and poor moisture resistance in particleboard are solved, and high moisture resistance and low formaldehyde emission are achieved, which is in line with the Multi-national standard particleboard requirements.

CN119039911APending Publication Date: 2024-11-29HENGSHUI BA MAI LONG WOOD CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411168155.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing urea formaldehyde resin has a high formaldehyde content in particleboard and lacks moisture-proof function, which causes particleboard to be easily damp in high humidity environments and may exceed the standard of formaldehyde, which endangers human health.

Method used

Modified urea-formaldehyde resin adhesive is used, which contains 26-40% formaldehyde, 23-38% urea, and 4-14% melamine, and carbon nanotubes-melamine cyanurate and sodium benzoate, and cross-links with urea-formaldehyde resin through melamine Form a three-dimensional network structure, reduce hydrophilic groups, combine moisture-proof agents to improve waterproof performance, and absorb formaldehyde through carbon nanotubes to reduce formaldehyde content.

Benefits of technology

It significantly improves the waterproof performance and thermal stability of particleboard, reduces formaldehyde emission, extends service life, and improves resistance to wood rot, mold and termites, and complies with the requirements of ENF and F**** standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention belongs to the technical field of composite artificial boards, and provides a urea-formaldehyde resin modified adhesive and application thereof in production of full-elm super-strong high-moisture-proof shaving boards, the urea-formaldehyde resin modified adhesive comprises the following raw materials by mass: 26-40% of formaldehyde, 23-18% of urea, and 4-14% of melamine; and the balance of auxiliaries. When the urea-formaldehyde resin modified adhesive provided by the invention is applied to a shaving board, the moisture resistance of the shaving board can be remarkably improved, the 24-hour water absorption thickness swelling rate is less than or equal to 5%, the wet static bending intensity is greater than or equal to 9.6 MPa, the formaldehyde emission is less than or equal to 0.020 mg / m < 3 > (climatic box method) and less than or equal to 0.20 mg / L (dryer method), and the urea-formaldehyde resin modified adhesive meets the requirements of China ENF-grade shaving boards and the requirements of Japanese national standard F * * * * *. And F * * * * / ENF dual authentication can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite artificial boards, in particular to a urea-formaldehyde resin modified adhesive and application thereof in the production of all-elm super-strong high moisture-proof particleboards. Background Art

[0002] Particleboard, also known as particle board, is a kind of man-made board made by cutting various branches, small-diameter wood, fast-growing wood, sawdust, etc. into pieces of certain specifications, drying them, mixing them with glue, hardener, waterproofing agent, etc., and pressing them under certain temperature and pressure. The particles are arranged unevenly. The particleboard industry has developed rapidly, but many companies do not pay attention to product quality, and there is a problem of serious formaldehyde exceeding the standard. In addition, traditional particleboard is susceptible to moisture and deformation in high humidity environments, which limits its widespread use in specific applications.

[0003] Urea-formaldehyde resin, also known as urea formaldehyde resin, is a urea-formaldehyde resin formed by the condensation of urea and formaldehyde under the action of a catalyst. It is widely used in the field of adhesives, especially in the wood processing industry and the manufacture of composite wood-based panels. However, urea-formaldehyde resin has poor water resistance and aging resistance because the cured resin contains hydrophilic free methylol groups, which are easily combined with water, thereby exacerbating the moisture-sensitive nature of particleboards. In addition, urea-formaldehyde resin also contains some formaldehyde, which can cause formaldehyde to exceed the standard in severe cases, endangering human health.

[0004] Therefore, in order to adapt to the different needs of society, there is an urgent need for a low-formaldehyde, moisture-proof urea-formaldehyde resin, which can be applied to particleboard materials to improve the moisture-proof performance of particleboard materials. Summary of the invention

[0005] The purpose of the present invention is to provide a urea-formaldehyde resin modified adhesive and its application in the production of all-elm super-strong high moisture-proof particleboard, so as to solve the problem that the urea-formaldehyde resin in the prior art has a high formaldehyde content and does not have a moisture-proof function when applied to the particleboard.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a urea-formaldehyde resin modified adhesive, comprising the following raw materials in percentage by mass:

[0008] Formaldehyde 26-40%, urea 23-38%, melamine 4-14%; the remainder is auxiliary agent.

[0009] Preferably, the auxiliary agent is selected from 2 to 4 parts of moisture-proof agent, 4 to 10 parts of carbon nanotube-melamine cyanurate, and 2 to 4 parts of sodium benzoate.

[0010] Preferably, the preparation method of carbon nanotube-melamine cyanurate is as follows:

[0011] 10 mg of carbon nanotubes were dispersed in 10 mL of a 0.01 g / L melamine cyanurate aqueous solution, the mixture was stirred evenly, and the solid was collected by centrifugation to obtain carbon nanotube-melamine cyanurate.

[0012] Preferably, in the urea-formaldehyde resin modified adhesive, the melamine is a cyclic melamine.

[0013] Preferably, the desiccant is OPE desiccant.

[0014] Preferably, the preparation method of the urea-formaldehyde resin modified adhesive comprises the following steps:

[0015] (1) adding formaldehyde to the reaction system, adjusting the pH of the reaction system to 7-8, adding the first portion of urea to react, and obtaining a first mixture after the reaction is completed;

[0016] (2) adding melamine to the first mixture and heating the mixture to a target temperature to react;

[0017] (3) After adjusting the pH of the reaction system in step (2) to 7-8, adding a second portion of urea to react to obtain a second mixture;

[0018] (4) dispersing the auxiliary agent in water to obtain a mixed dispersion, and mixing the mixed dispersion with the second mixture to obtain the urea-formaldehyde resin modified adhesive.

[0019] Preferably, the reaction temperature in step (1) is 40-50° C., and the reaction time is 5-15 min.

[0020] Preferably, the target temperature in step (2) is 80-90° C., and the reaction time is 30-50 min.

[0021] Preferably, the reaction temperature in step (3) is 80-90° C., and the reaction time is 60-70 min.

[0022] Preferably, the first portion of urea and the second portion of urea are added in equal amounts.

[0023] The present invention also provides the use of any of the urea-formaldehyde resin modified adhesives in the production of all-elm super-strong high moisture-proof particleboards.

[0024] Preferably, in the all-elm super-strong and moisture-proof particleboard, the urea-formaldehyde resin modified adhesive is added to the core layer and the surface layer particles respectively; the added amount of the urea-formaldehyde resin modified adhesive accounts for 18.2% of the total mass of the board.

[0025] The present invention has the following beneficial effects:

[0026] The present invention provides a urea-formaldehyde resin modified adhesive, comprising the following raw materials in percentage by mass: 26-40% formaldehyde, 13-18% urea, 4-14% melamine; the remainder is an auxiliary agent. The present invention adopts melamine to modify the urea-formaldehyde resin, wherein the melamine can react with the hydroxymethyl urea in the urea-formaldehyde resin to reduce the number of hydrophilic groups (such as hydroxyl and amino groups), thereby improving the water resistance of the resin. In addition, the melamine with a ring structure can effectively cross-link with the urea-formaldehyde resin to form a three-dimensional network structure, which has a sealing effect on some hydrophilic groups and further enhances water resistance; after coordinating with a moisture-proof agent, the waterproof performance of the adhesive is significantly improved, thereby giving the particleboard moisture resistance. The present invention also adds carbon nanotubes, which have a large specific surface area and a special hollow tubular structure. First, they can accommodate the added melamine urate, and second, they can effectively absorb free formaldehyde in urea-formaldehyde resin, thereby reducing the formaldehyde content. Third, the combination of the two can better absorb formaldehyde, making the prepared particleboard more environmentally friendly.

[0027] The melamine urate added in the present invention can also improve the thermal stability of the adhesive and enhance the flame retardant performance. Sodium benzoate improves the corrosion resistance of the adhesive, prolongs the service life of the particleboard, and has good resistance to wood decay fungi, molds and termites.

[0028] The present invention also provides the use of the urea-formaldehyde resin modified adhesive in the production of all-elm super-strong high moisture-proof particleboard. After the urea-formaldehyde resin modified adhesive provided by the present invention is applied to the particleboard, the wet static bending strength is ≥9.6MPa, the 24h water absorption thickness expansion rate is ≤5%, and the formaldehyde release is ≤0.020mg / m 3 (climate chamber method), formaldehyde emission ≤ 0.20mg / L (dryer method) meets the requirements of China's national ENF grade particleboard and Japan's national standard F****, and can achieve F**** / ENF dual certification. DETAILED DESCRIPTION

[0029] The present invention provides a urea-formaldehyde resin modified adhesive, comprising the following raw materials in percentage by mass:

[0030] Formaldehyde 26-40%, urea 23-38%, melamine 4-14%; the remainder is auxiliary agent.

[0031] In the present invention, the mass percentage of formaldehyde is preferably 30 to 35%, more preferably 31 to 34%, and even more preferably 32 to 33%.

[0032] In the present invention, the mass percentage of urea is preferably 24-27%, more preferably 25-26%, and more preferably 25.5%.

[0033] In the present invention, the mass percentage of melamine is preferably 5 to 13%, more preferably 7 to 11%, and even more preferably 9%.

[0034] In the present invention, the auxiliary agent is selected from 2 to 4 parts of moisture-proof agent, 4 to 10 parts of carbon nanotube-melamine cyanurate, and 2 to 4 parts of sodium benzoate.

[0035] In the present invention, the mass fraction of the moisture-proofing agent is preferably 2.5 to 3.5 parts, more preferably 2.7 to 3.2 parts, and even more preferably 3 parts.

[0036] In the present invention, the mass fraction of the carbon nanotube-melamine cyanurate is preferably 5.5 to 8.5 parts, more preferably 6.3 to 7.7 parts, and even more preferably 7 parts.

[0037] In the present invention, the mass fraction of the sodium benzoate is preferably 2.5 to 3.5 parts, more preferably 2.5 to 3.2 parts, and more preferably 3 parts.

[0038] In the present invention, the melamine is preferably melamine with a ring structure.

[0039] In the present invention, the desiccant is preferably an OPE desiccant.

[0040] In the present invention, the preparation method of the urea-formaldehyde resin modified adhesive comprises the following steps:

[0041] (1) adding formaldehyde to the reaction system, adjusting the pH of the reaction system to 7-8, adding the first portion of urea to react, and obtaining a first mixture after the reaction is completed;

[0042] (2) adding melamine to the first mixture and heating the mixture to a target temperature to react;

[0043] (3) After adjusting the pH of the reaction system in step (2) to 7-8, adding a second portion of urea to react to obtain a second mixture;

[0044] (4) dispersing the auxiliary agent in water to obtain a mixed dispersion, and mixing the mixed dispersion with the second mixture to obtain the urea-formaldehyde resin modified adhesive.

[0045] In the present invention, the reaction temperature in step (1) is preferably 40-50°C, more preferably 42-48°C, more preferably 44-46°C, and the reaction time is preferably 5-15 min, more preferably 8-12 min, more preferably 10 min.

[0046] In the present invention, the target temperature in step (2) is preferably 80-90°C, more preferably 82-88°C, more preferably 84-86°C, and the reaction time is preferably 30-50 min, more preferably 35-45 min, more preferably 38-42 min.

[0047] In the present invention, the reaction temperature in step (3) is preferably 80-90°C, more preferably 82-88°C, more preferably 84-86°C, and the reaction time is preferably 60-70 min, more preferably 62-68°C, more preferably 64-66°C.

[0048] In the present invention, the first portion of urea and the second portion of urea are added in equal amounts.

[0049] The present invention also provides the use of the urea-formaldehyde resin modified adhesive in the production of all-elm super-strong high moisture-proof particleboard.

[0050] In the present invention, in the all-elm super-strong high moisture-proof particleboard, the core layer and the surface layer particles are respectively added with the urea-formaldehyde resin modified adhesive; the addition amount of the urea-formaldehyde resin modified adhesive accounts for 18.2% of the total mass of the board.

[0051] The present invention also provides a method for preparing the all-elm super-strong high moisture-proof particleboard, comprising the following steps:

[0052] Fully peeled elm is used to plane shavings with a thickness of 0.4mm, a length of 45mm, and a length-to-thickness ratio of 112, accounting for 20%, and shavings with a thickness of 0.6mm, a length of 45mm, and a length-to-thickness ratio of 75, accounting for 30%. The urea glue application amount is 100kg / cubic meter, the paraffin addition amount is 8kg / cubic meter, and the formaldehyde reducing agent addition amount is 1kg / cubic meter. The slabs are passed through a paving machine and a continuous flat press to produce a three-layer gradient structure particleboard.

[0053] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0054] Example 1

[0055] A urea-formaldehyde resin modified adhesive comprises the following raw materials in parts by weight:

[0056] 35 parts of formaldehyde, 28 parts of urea, 8 parts of melamine, and 29 parts of additives.

[0057] The auxiliary agent is selected from 4 parts of OPE moisture-proof agent, 6 parts of carbon nanotube-melamine cyanurate, and 2 parts of sodium benzoate.

[0058] (1) adding formaldehyde to the reaction system, adjusting the pH of the reaction system to 7, adding the first portion of urea and reacting at a temperature of 40° C. for 5 minutes, and obtaining a first mixture after the reaction is completed;

[0059] (2) adding melamine to the first mixture, heating to 80° C. and reacting for 30 minutes;

[0060] (3) After adjusting the pH of the reaction system in step (2) to 7, adding a second portion of urea, and reacting at a temperature of 80° C. for 60 minutes to obtain a second mixture;

[0061] (4) Dispersing the OPE moisture-proof agent, carbon nanotube-melamine urate, and sodium benzoate in 27 parts of water to obtain a mixed dispersion, and mixing the mixed dispersion with the second mixture to obtain the urea-formaldehyde resin modified adhesive.

[0062] The urea-formaldehyde resin modified adhesive obtained in this example is applied to the all-elm super-strong high moisture-proof particleboard.

[0063] The core layer and the surface layer wood chips are respectively added with urea-formaldehyde resin modified adhesive; the added amount of the urea-formaldehyde resin modified adhesive accounts for 18.2% of the total mass of the board.

[0064] Example 2

[0065] A urea-formaldehyde resin modified adhesive comprises the following raw materials in parts by weight:

[0066] 40 parts of formaldehyde, 38 parts of urea, 10 parts of melamine, and 12 parts of additives.

[0067] The auxiliary agent is selected from 3 parts of OPE moisture-proof agent, 9 parts of carbon nanotube-melamine cyanurate, and 4 parts of sodium benzoate.

[0068] (1) adding formaldehyde to the reaction system, adjusting the pH of the reaction system to 7, adding the first portion of urea and reacting at a temperature of 50° C. for 15 minutes, and obtaining a first mixture after the reaction is completed;

[0069] (2) adding melamine to the first mixture, heating to 90° C. and reacting for 50 minutes;

[0070] (3) After adjusting the pH of the reaction system in step (2) to 8, a second portion of urea was added, and the mixture was reacted at 90° C. for 70 min to obtain a second mixture;

[0071] (4) Dispersing the OPE moisture-proof agent, carbon nanotube-melamine cyanurate, and sodium benzoate in 16 parts of water to obtain a mixed dispersion, and mixing the mixed dispersion with the second mixture to obtain the urea-formaldehyde resin modified adhesive.

[0072] The urea-formaldehyde resin modified adhesive obtained in this example is applied to the all-elm super-strong high moisture-proof particleboard.

[0073] The core layer and the surface layer wood chips are respectively added with urea-formaldehyde resin modified adhesive; the added amount of the urea-formaldehyde resin modified adhesive accounts for 18.2% of the total mass of the board.

[0074] Example 3

[0075] A urea-formaldehyde resin modified adhesive comprises the following raw materials in parts by weight:

[0076] 38 parts of formaldehyde, 37 parts of urea, 12 parts of melamine, and 13 parts of additives.

[0077] The auxiliary agent is selected from 3 parts of OPE moisture-proof agent, 9 parts of carbon nanotube-melamine cyanurate, and 4 parts of sodium benzoate.

[0078] (1) adding formaldehyde to the reaction system, adjusting the pH of the reaction system to 7, adding the first portion of urea and reacting at a temperature of 45° C. for 15 minutes, and obtaining a first mixture after the reaction is completed;

[0079] (2) adding melamine to the first mixture, heating to 88° C. and reacting for 45 minutes;

[0080] (3) After adjusting the pH of the reaction system in step (2) to 8, adding a second portion of urea, and reacting at a temperature of 85° C. for 65 minutes to obtain a second mixture;

[0081] (4) Dispersing the OPE moisture-proof agent, carbon nanotube-melamine cyanurate, and sodium benzoate in 17 parts of water to obtain a mixed dispersion, and mixing the mixed dispersion with the second mixture to obtain the urea-formaldehyde resin modified adhesive.

[0082] The urea-formaldehyde resin modified adhesive obtained in this example is applied to the all-elm super-strong high moisture-proof particleboard.

[0083] The core layer and the surface layer wood chips are respectively added with urea-formaldehyde resin modified adhesive; the added amount of the urea-formaldehyde resin modified adhesive accounts for 18.2% of the total mass of the board.

[0084] Example 4

[0085] A urea-formaldehyde resin modified adhesive comprises the following raw materials in parts by weight:

[0086] 30 parts of formaldehyde, 28 parts of urea, 13 parts of melamine, and 29 parts of additives.

[0087] The auxiliary agent is selected from 2 parts of OPE moisture-proof agent, 10 parts of carbon nanotube-melamine cyanurate, and 4 parts of sodium benzoate.

[0088] (1) adding formaldehyde to the reaction system, adjusting the pH of the reaction system to 7, adding the first portion of urea and reacting at a temperature of 45° C. for 15 minutes, and obtaining a first mixture after the reaction is completed;

[0089] (2) adding melamine to the first mixture, heating to 85° C. and reacting for 40 minutes;

[0090] (3) After adjusting the pH of the reaction system in step (2) to 8, a second portion of urea was added, and the mixture was reacted at 90° C. for 70 min to obtain a second mixture;

[0091] (4) Dispersing the OPE moisture-proof agent, carbon nanotube-melamine cyanurate, and sodium benzoate in 17 parts of water to obtain a mixed dispersion, and mixing the mixed dispersion with the second mixture to obtain the urea-formaldehyde resin modified adhesive.

[0092] The urea-formaldehyde resin modified adhesive obtained in this example is applied to the all-elm super-strong high moisture-proof particleboard.

[0093] The core layer and the surface layer wood chips are respectively added with urea-formaldehyde resin modified adhesive; the added amount of the urea-formaldehyde resin modified adhesive accounts for 18.2% of the total mass of the board.

[0094] Example 5

[0095] A urea-formaldehyde resin modified adhesive comprises the following raw materials in parts by weight:

[0096] 39 parts of formaldehyde, 26 parts of urea, 13 parts of melamine, and 22 parts of additives.

[0097] The auxiliary agent is selected from 4 parts of OPE moisture-proof agent, 9 parts of carbon nanotube-melamine cyanurate, and 3 parts of sodium benzoate.

[0098] (1) adding formaldehyde to the reaction system, adjusting the pH of the reaction system to 7, adding the first portion of urea and reacting at a temperature of 45° C. for 12 minutes, and obtaining a first mixture after the reaction is completed;

[0099] (2) adding melamine to the first mixture, heating to 86° C. and reacting for 46 minutes;

[0100] (3) After adjusting the pH of the reaction system in step (2) to 7, a second portion of urea was added, and the mixture was reacted at 88° C. for 62 min to obtain a second mixture;

[0101] (4) Dispersing the OPE moisture-proof agent, carbon nanotube-melamine cyanurate, and sodium benzoate in 17 parts of water to obtain a mixed dispersion, and mixing the mixed dispersion with the second mixture to obtain the urea-formaldehyde resin modified adhesive.

[0102] The urea-formaldehyde resin modified adhesive obtained in this example is applied to the all-elm super-strong high moisture-proof particleboard.

[0103] The core layer and the surface layer wood chips are respectively added with urea-formaldehyde resin modified adhesive; the added amount of the urea-formaldehyde resin modified adhesive accounts for 18.2% of the total mass of the board.

[0104] Performance Testing

[0105] The particleboards obtained in Examples 1 to 5 were tested for their physical and mechanical properties according to GB / T 4897-2015, and the formaldehyde emission was determined according to the climate chamber method in GB / T 39600-2021. In addition, the free formaldehyde emission was determined according to the dryer method in JIS A1460:2021. The wet static bending strength was determined according to the determination method A specified in 6.12 of GB / T11718-2009. The specific test results are shown in Table 1.

[0106] Table 1 Particleboard performance test results obtained in Examples 1 to 5

[0107]

[0108]

[0109] It can be seen from Table 1 that the urea-formaldehyde resin modified adhesive provided by the present invention can significantly improve the moisture resistance of the particle board after being applied to the particle board, the 24h water absorption thickness expansion rate is ≤5%, the wet static bending strength is ≥9.6MPa, and the formaldehyde release is ≤0.020mg / m 3 (climate chamber method), formaldehyde emission ≤0.20mg / L (dryer method) meets the requirements of China's national ENF grade particleboard and Japan's national standard F****, and can achieve F**** / ENF dual certification.

[0110] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A urea-formaldehyde resin modified adhesive, characterized in that: Contains the following raw materials in percentage by weight: Formaldehyde 26-40%, urea 23-38%, melamine 4-14%; the remainder is auxiliary agent.

2. The urea-formaldehyde resin modified adhesive according to claim 1, characterized in that: The auxiliary agent is selected from 2 to 4 parts of moisture-proof agent, 6 to 10 parts of carbon nanotube-melamine cyanurate, and 2 to 4 parts of sodium benzoate.

3. The urea-formaldehyde resin modified adhesive according to claim 1, characterized in that: The melamine is a melamine with a ring structure.

4. The urea-formaldehyde resin modified adhesive according to claim 1, characterized in that: The preparation method of the urea-formaldehyde resin modified adhesive comprises the following steps: (1) adding formaldehyde to the reaction system, adjusting the pH of the reaction system to 7-8, adding the first portion of urea to react, and obtaining a first mixture after the reaction is completed; (2) adding melamine to the first mixture and heating the mixture to a target temperature to react; (3) After adjusting the pH of the reaction system in step (2) to 7-8, adding a second portion of urea to react to obtain a second mixture; (4) dispersing the auxiliary agent in water to obtain a mixed dispersion, and mixing the mixed dispersion with the second mixture to obtain the urea-formaldehyde resin modified adhesive.

5. The urea-formaldehyde resin modified adhesive according to claim 4, characterized in that: The reaction temperature in step (1) is 40-50° C., and the reaction time is 5-15 min.

6. The urea-formaldehyde resin modified adhesive according to claim 4 or 5, characterized in that: The target temperature in step (2) is 80-90° C., and the reaction time is 30-50 min.

7. The urea-formaldehyde resin modified adhesive according to claim 4 or 5, characterized in that: The reaction temperature in step (3) is 80-90° C., and the reaction time is 60-70 min.

8. The urea-formaldehyde resin modified adhesive according to claim 4, characterized in that: The first urea and the second urea are added in equal amounts.

9. Use of the urea-formaldehyde resin modified adhesive according to any one of claims 1 to 8 in the production of all-elm super-strong and moisture-proof particleboard.

10. The use of the urea-formaldehyde resin modified adhesive as claimed in claim 9 in the production of all-elm super-strong high moisture-proof particleboard, characterized in that: In the all-elm super-strong moisture-proof particleboard, the core layer and the surface layer particles are respectively added with the urea-formaldehyde resin modified adhesive described in any one of claims 1 to 8; the addition amount of the urea-formaldehyde resin modified adhesive accounts for 18.2% of the total mass of the board.

Citation Information

Cited By

  • Method for producing moisture-proof health-preserving shaving board based on elm as raw material and process for controlling length-to-thickness ratio of flakes

    CN120816582A