Polyurethane adhesive and method for producing polyurethane adhesive
Through the ratio and process of solvent-free polyurethane adhesive, the problem of poor adhesive peeling performance in products such as lightweight conveyor belts and tarps is solved, and high mechanical performance and environmental protection are achieved. It is suitable for a variety of industries and Construction field.
Patent Information
- Application Number
- CN202411294913.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The poor peeling performance of adhesives in existing light-duty conveyor belts and tarps have resulted in reduced mechanical properties of the product, easy to absorb moisture, and affecting service life. The traditional polyurethane adhesive contains organic solvents that pose a threat to the environment and human health.
Using solvent-free polyurethane adhesive, the raw material ratio is diisocyanate, benzoate, polyester polyol, catalyst, stabilizer and water removal agent, polymerization reaction is carried out through specific process steps to form high reaction activity and Chemical bonds improve the mechanical adhesion and weather resistance of the adhesive.
It achieves high tear strength, peel strength and tensile strength, extends service life, complies with environmental protection standards, avoids the harm of traditional adhesives to the environment and the human body, and is suitable for a variety of industrial and construction fields.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, in particular to a polyurethane adhesive and a method for preparing the polyurethane adhesive. Background Art
[0002] At present, the market demand for products such as light conveyor belts, waterproof fabrics, car tarpaulins, structural membranes, and inflatable materials continues to grow. With the further advancement of industrialization and urbanization, these products have become an important part of industrial production and life. In particular, conveyor belts are widely used in many industries such as logistics and machinery manufacturing. Waterproof fabrics are widely used in the construction industry, especially in the field of new environmentally friendly building materials, which has great market potential. Car tarpaulins are important auxiliary materials for the modern automobile industry. According to market research, products such as conveyor belts, waterproof fabrics, and car tarpaulins have a high market penetration rate and have become standard equipment for many related industries. It can be reasonably predicted that this industry still has great development prospects.
[0003] Light conveyor belts are widely used in food, medicine, electronics, tobacco, printing, packaging, wood, textiles, building materials, transportation, postal services, logistics and other industries for the transmission of goods, bags, bulk materials, as well as in factory internal production flow operations and agricultural and sideline product processing.
[0004] At present, as one of the three major technical indicators of light conveyor belts, anti-peeling performance plays an important role in the performance of the product. Existing products have the disadvantage of poor peeling performance. As time goes by, poor adhesion often occurs, and even the matrix and the matrix are separated. This results in reduced mechanical properties of the product, easy moisture absorption, and seriously affects its service life.
[0005] In the textile industry, textiles for sails are mainly used in the fields of warehousing, transportation, advertising, etc. Textiles for sails can be used as waterproof awnings. When used in warehousing, freight and other places, this textile can better cover the surface of objects and has the functions of corrosion resistance, waterproofness and fire resistance; Textiles for national defense: mainly used in military, aerospace, and national defense construction, including parachutes, aerospace textiles and textiles for soldiers; Textiles for entertainment: mainly used for outdoor awnings, inflatable castles, inflatable surfboards, outdoor tents, etc.
[0006] In the above-mentioned textile industries, the adhesives used also have the problem of poor peeling performance. Therefore, a polyurethane adhesive and a method for preparing the polyurethane adhesive are proposed to solve this problem.
[0007] Moreover, the polyurethane adhesive does not contain solvents and has little harm to the environment and human body, which is different from most polyurethane adhesives containing solvents on the market (such as containing ethyl acetate, butanone, etc. as solvents, and having a high solid content).
[0008] In the current market, polyurethane adhesives are widely used in various industrial and construction fields. However, these adhesives usually contain a large amount of organic solvents such as ethyl acetate, butanone, toluene and butyl acetate. Although these solvents can effectively reduce the viscosity of the adhesive, their volatility poses a potential threat to human health during use. Long-term exposure to these volatile organic compounds may cause headaches, respiratory diseases, and even increase the risk of cancer. Using benzoate plasticizers and not using organic solvents as raw materials for polyurethane adhesives is a more environmentally friendly choice. Benzoate is an environmentally friendly non-toxic plasticizer, which has better safety and environmental friendliness than phthalate plasticizers commonly used in traditional adhesives (such as dibutyl phthalate DBP, butyl benzyl phthalate BBP, di (2-ethylhexyl) phthalate DEHP, diisononyl phthalate DINP and diisodecyl phthalate DIDP). These phthalate plasticizers have been confirmed by a large number of studies to be potentially toxic to reproductive development, and this risk has been more widely recognized in recent years. Therefore, with the continuous improvement of people's living standards and the increasing awareness of environmental protection, it has become a general trend to use environmentally friendly and non-toxic plasticizers to replace traditional phthalates. Summary of the invention
[0009] The purpose of the present invention is to provide a polyurethane adhesive and a method for producing the polyurethane adhesive, which solves the problem of poor peelability in the current use of light conveyor belts and waterproof cloth industries.
[0010] To achieve the above object, the present invention provides the following technical solution: polyurethane adhesive, the raw material ratio is as follows:
[0011] 10-40 parts of diisocyanate, 40-80 parts of plasticizer benzoate, 0-40 parts of polyester polyol, 1-3 parts of catalyst, 3-5 parts of stabilizer and 1-5 parts of water remover.
[0012] Preferably, the diisocyanate is one or more of toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI) and isophorone diisocyanate (IPDI).
[0013] Preferably, the benzoic acid ester is one or more of methyl benzoate, ethyl benzoate, propyl benzoate, butyl benzoate, isopropyl benzoate, benzyl benzoate, isobutyl benzoate, pentyl benzoate, isopentyl benzoate, hexyl benzoate, and diethylene glycol dibenzoate.
[0014] Preferably, the polyester polyol is one or more of adipic acid polyester diol, aromatic polyester polyol, dimer polyester diol, polycaprolactone polyol, polycarbonate diol, and special polyester polyol with side groups;
[0015] The functionality of the polyester polyol is 1.5-2, and the number average molecular weight is 1000-1500 g / mol.
[0016] Preferably, the catalyst is specifically one of an organic metal catalyst and an amine catalyst;
[0017] The organometallic catalyst includes one of dibutyltin dilaurate, stannous octoate, dibutyltin diacetate, calcium isooctanoate, zinc isooctanoate, bismuth isooctanoate, sodium isooctanoate or a mixture thereof;
[0018] The amine catalyst is selected from one or a mixture of N,N-dimethylcyclohexane, triethylenediamine, N,N,N,N-tetramethylalkylenediamine, N,N,N,N-pentamethyldiethylenetriamine, triethylamine, N,N-dimethylbenzylamine, N,N-dimethylhexadecylamine, N,N-dimethylbutylamine, and 2,2'-dimorpholinodiethyl ether.
[0019] Preferably, the stabilizer is trisnonylphenyl phosphite, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate and methyl 1, triphenyl phosphite, 2-(2-hydroxy-3,5-di-tert-butylphenyl)-5-chlorobenzotriazole and a mixture thereof.
[0020] Preferably, the dehydrating agent is one or more of calcium oxide, 4A molecular sieve and calcium carbonate.
[0021] The method for preparing a polyurethane adhesive comprises the following steps:
[0022] The dehumidifier was dried at 200°C for about 20 hours and then cooled in a sealed container;
[0023] Put polyester polyol and benzoate into a reaction kettle;
[0024] The mixture was degassed, then maintained at 50°C under vacuum and mixed uniformly, nitrogen was introduced to break the vacuum and then stabilizer was added, followed by additional degassing and mixing under vacuum, diisocyanate was added under nitrogen protection and mixed, 1% of the total amount of the catalyst was added dropwise, polymerization occurred in the autoclave and the temperature was raised to 120;
[0025] The reaction mixture was maintained at 80°C to 90°C for 30 minutes by physical cooling, and then cooled to 60°C. After drying and dehydrating agent was added, the mixture was cooled to room temperature and then discharged and packaged.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The test results of cadmium, lead, mercury, phthalates, butyl benzyl phthalate, diisobutyl phthalate, etc. in the patent of the present invention all comply with the amendment directive of Annex II of the EU RoHS Directive 2011 / 65EU and the limit requirements of (EU) 2015 / 863.
[0028] The adhesive of the present invention is widely used in PVC paste resin, for coating polyester and nylon fibers, and is mainly used in the production and processing of waterproof tarpaulins and light conveyor belts. The fiber has a rough open surface, is easy to be penetrated by the slurry, and has good mechanical adhesion after plasticization.
[0029] The adhesive also has a long service life and open time.
[0030] The patent of the present invention complies with environmental protection requirements and is a pure environmentally friendly product without adding any phthalate plasticizers. The patent of the present invention can meet the EU national standards. Compared with other products on the market, when the base fabric specifications, sizing ratio, temperature, ratio and other process parameters are the same, the manufactured product has high tear strength, peel strength, tensile strength, and is not easy to age and fade under different weather conditions.
[0031] Furthermore, the polyurethane adhesive does not contain any solvent and has little harm to the environment and human body. DETAILED DESCRIPTION
[0032] The present invention will be described in more detail below by way of examples, which are merely illustrative and do not in any way limit the scope of the present invention.
[0033] In one aspect of the present invention, the present invention provides a technical solution: a polyurethane adhesive, wherein the raw material ratio is as follows:
[0034] 10-40 parts of diisocyanate, 40-80 parts of plasticizer benzoate, 0-40 parts of polyester polyol, 1-3 parts of catalyst, 3-5 parts of stabilizer and 1-5 parts of water remover.
[0035] According to an embodiment of the present invention, the diisocyanate is one or more of toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI) and isophorone diisocyanate (IPDI). According to an embodiment of the present invention, the polymer of diisocyanate and polyol is applied to the adhesive to show its high reactivity, strong chemical bond and physical bond formation; diisocyanate has high reactivity and can form covalent bonds with many adhered materials containing active hydrogen atoms on the surface, such as metal, rubber, fiber, plastic, etc. The combined effect of this chemical adhesion and physical adhesion makes the adhered substrates produce very high bonding strength, which is suitable for use in the textile industry; Strong chemical bond and physical bond formation: Isocyanate is a type of substance containing isocyanate group (-NCO) and carbamate group (-NHCOO-) in the molecular chain, has high polarity and activity, and can form strong chemical bonds and physical bonds with various materials including active hydrogen. This bonding strength is extremely high and is particularly suitable for bonding engineering plastics to base fabrics.
[0036] According to an embodiment of the present invention, the benzoic acid ester is one or more of methyl benzoate, ethyl benzoate, propyl benzoate, butyl benzoate, isopropyl benzoate, isobutyl benzoate, pentyl benzoate, isopentyl benzoate, hexyl benzoate and benzyl benzoate. According to an embodiment of the present invention, the benzoic acid ester is a plasticizer with low toxicity and is environmentally friendly. It is used to reduce the viscosity of the adhesive and is added to the adhesive to have the characteristics of low volatility, oil resistance, water resistance, light resistance, good pollution resistance, etc.
[0037] According to an embodiment of the present invention, the polyester polyol is one or more of adipic acid-based polyester diol, aromatic polyester polyol, dimer polyester diol, polycaprolactone polyol, polycarbonate diol, and special polyester polyol with side groups; the functionality of the polyester polyol is 1.5-2, and the number average molecular weight is 1000-1500 g / mol. According to an embodiment of the present invention, the polyester polyol has a relatively long molecular chain structure and polyhydroxy functional groups, and can form a high molecular weight polyurethane network by reacting with isocyanate. This structure enables the adhesive to have excellent mechanical properties and bonding strength.
[0038] According to an embodiment of the present invention, the catalyst is specifically one of an organic metal catalyst and a tertiary amine catalyst; the organic metal catalyst includes one or more of dibutyltin dilaurate, stannous octoate, dibutyltin diacetate, calcium isooctanoate, zinc isooctanoate, bismuth isooctanoate, and sodium isooctanoate; the amine catalyst is selected from N,N dimethylcyclohexane, triethylenediamine, N,N,N,N-tetramethylalkylenediamine, N,N,N,N-pentamethyldiethylenetriamine, triethylamine, N,N-dimethylbenzylamine, N,N-dimethylhexadecylamine, N,N-dimethylbutylamine, 2,2'-dimorpholinodiethyl ether or a mixture of these; according to an embodiment of the present invention, the application of the catalyst is to accelerate the polymerization reaction of diisocyanate and polyester polyol.
[0039] According to an embodiment of the present invention, the stabilizer is trinonylphenyl phosphite, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate and methyl 1, triphenyl phosphite, 2-(2-hydroxy-3,5-di-tert-butylphenyl)-5-chlorobenzotriazole and a mixture of these; it is mainly used in the present invention to prevent the polyurethane adhesive from thermally degrading under high temperature and ultraviolet irradiation, and to inhibit the oxidation reaction of the adhesive with air.
[0040] According to an embodiment of the present invention, the dehydrating agent is one or more of calcium oxide, 4A molecular sieve and calcium carbonate. According to an embodiment of the present invention, the application of the dehydrating agent can remove excess moisture in the adhesive and reduce the impact of moisture on product quality.
[0041] Preparation method
[0042] Embodiment 1:
[0043] The dehydrating agent calcium carbonate is dried at 200°C for about 20 hours and then cooled in a sealed container;
[0044] 5% by weight of polybutylene terephthalate (molecular weight 1000) and 65% by weight of benzyl benzoate were charged into a reaction kettle;
[0045] The mixture was degassed, then maintained at 50° C. under vacuum and mixed uniformly, nitrogen was introduced to break the vacuum and then 3 parts of trisnonylphenyl phosphite, a stabilizer, was added, followed by further degassing and mixing under vacuum, 30% of the total weight of toluene diisocyanate was added under nitrogen protection and mixed uniformly, 1 part of the catalyst triethylenediamine was added dropwise, a polymerization reaction occurred in the kettle and the temperature was raised to 120° C.;
[0046] The reaction mixture was cooled physically and maintained between 80°C and 90°C for 30 minutes. The reaction mixture was then cooled to 60°C, and 5 parts of dried dehydrating agent calcium carbonate were added, and the mixture was cooled to room temperature before being discharged and packaged.
[0047] Embodiment 2:
[0048] Dry the dehydrating agent 4A grade molecular sieve at 200°C for about 20 hours and then cool it in a sealed container;
[0049] 50% by weight of benzyl benzoate and 10% by weight of diphenylmethane diisocyanate are charged into a reaction kettle;
[0050] The mixture was degassed, and then maintained at 80° C.-90° C. under vacuum to mix uniformly, nitrogen was introduced to break the vacuum and 40% of the total weight of polyethylene terephthalate was slowly added dropwise, followed by further degassing and mixing under vacuum, and 2 parts of the catalyst dibutyltin dilaurate were added dropwise under nitrogen protection to react, and a polymerization reaction occurred in the kettle and the temperature was raised to 170° C.;
[0051] The reaction mixture was maintained at 80°C to 90°C for 30 minutes by physical cooling. The reaction mixture was then cooled to 60°C, and 3 portions of dried dehydrating agent 4A molecular sieve were added, and the mixture was cooled to room temperature before being discharged and packaged.
[0052] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. Polyurethane adhesive, Features: The raw material ratio is as follows: 10-40 parts of diisocyanate, 40-80 parts of plasticizer benzoate, 0-40 parts of polyester polyol, 1-3 parts of catalyst, 3-5 parts of stabilizer and 1-5 parts of water remover.
2. The polyurethane adhesive according to claim 1, Features: The diisocyanate is one or more of toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI) and isophorone diisocyanate (IPDI).
3. The polyurethane adhesive according to claim 1, Features: The benzoic acid ester is one or more of methyl benzoate, ethyl benzoate, propyl benzoate, butyl benzoate, isopropyl benzoate, isobutyl benzoate, pentyl benzoate, isopentyl benzoate, benzyl benzoate, hexyl benzoate and diethylene glycol dibenzoate.
4. The polyurethane adhesive according to claim 1, Features: The polyester polyol is one or more of adipic acid polyester diol, aromatic polyester polyol, dimer polyester diol, polycaprolactone polyol, polycarbonate diol, and special polyester polyol with side groups; The functionality of the polyester polyol is 1.5-2, and the number average molecular weight is 1000-1500 g / mol.
5. The polyurethane adhesive according to claim 1, Features: The catalyst is specifically one of an organic metal catalyst and an amine catalyst; The organometallic catalyst includes one of dibutyltin dilaurate, stannous octoate, dibutyltin diacetate, calcium isooctanoate, zinc isooctanoate, bismuth isooctanoate and sodium isooctanoate, or a mixture thereof; The amine catalyst is selected from one or a mixture of N,N-dimethylcyclohexane, triethylenediamine, N,N,N,N-tetramethylalkylenediamine, N,N,N,N-pentamethyldiethylenetriamine, triethylamine, N,N-dimethylbenzylamine, N,N-dimethylhexadecylamine, N,N-dimethylbutylamine, and 2,2'-dimorpholinodiethyl ether.
6. The polyurethane adhesive according to claim 1, Features: The dehydrating agent is one or more of calcium oxide, 4A molecular sieve and calcium carbonate.
7. The polyurethane adhesive according to claim 1, Features: The stabilizer is trisnonylphenyl phosphite, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate and methyl 1, triphenyl phosphite, 2-(2-hydroxy-3,5-di-tert-butylphenyl)-5-chlorobenzotriazole and a mixture of these.
8. A method for producing a polyurethane adhesive according to any one of claims 1 to 7, Features: The following steps are involved: The dehumidifier was dried at 200°C for about 20 hours and then cooled in a sealed container; Put polyester polyol and benzoate into a reaction kettle; The mixture was degassed, then mixed uniformly under vacuum at 50°C, nitrogen was introduced to break the vacuum and then stabilizer was added, followed by additional degassing and mixing under vacuum, diisocyanate was added and mixed under nitrogen protection, 1% of the total amount of the catalyst was added dropwise, polymerization occurred in the autoclave and the temperature was raised to 120°C; The reaction mixture was maintained at 80°C to 90°C for 30 minutes by physical cooling, and then cooled to 60°C. After drying and dehydrating agent was added, the mixture was cooled to room temperature and then discharged and packaged.