Spectral selective solar phase change heat storage material and preparation method thereof

By combining porous silicon carbide material and plasma nanometal foil in solar phase change heat storage materials, the problem of high infrared emissivity under high temperature conditions is solved, and efficient solar heat storage effect is achieved.

CN119039944AActive Publication Date: 2024-11-29NANJING UNIV OF AERONAUTICS & ASTRONAUTICS
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411254908.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-08-16
Filing Date
2024-09-09
Publication Date
2024-11-29
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

The existing solar phase change heat storage materials have high infrared emissivity under high temperature conditions, resulting in serious heat loss and affecting the solar heat storage efficiency.

Method used

Using spectral selective solar phase change heat storage material composed of porous silicon carbide material and plasma nanometal foil, the porous silicon carbide material is filled with bisea tetrapentanol and superimposed zinc foil on its surface to improve the Spectral absorption and suppress infrared emissivity.

Benefits of technology

It significantly improves the solar phase change heat storage efficiency, reduces infrared radiation loss, and improves the heat storage and release capacity of the material under high temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039944A_ABST
    Figure CN119039944A_ABST
Patent Text Reader

Abstract

The invention discloses a solar phase change heat storage material with spectral selectivity and a preparation method thereof, the material is composed of two layers of materials, the bottom layer is a porous silicon carbide material filled with a phase change material, and the top layer is a plasma nano metal foil; the preparation method comprises the following steps: (1) filling the porous silicon carbide material with the phase change material; and (2) superposing the plasma nano metal foil on the upper surface of the porous silicon carbide material filled with the phase change material. According to the invention, the porous silicon carbide material filled with the phase change material is combined with the plasma nano metal foil, so that the absorption efficiency in a solar spectrum range is improved, and meanwhile, the infrared radiation loss is inhibited.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an energy storage material and a preparation method thereof, and in particular to a spectrally selective solar energy phase change heat storage material and a preparation method thereof. Background Art

[0002] As global energy demand continues to grow and environmental problems become increasingly severe, the development of efficient and environmentally friendly energy storage technology has become the focus of current research. As a clean and renewable energy source, solar energy has broad application prospects. However, how to efficiently capture, store and utilize solar energy remains an important technical challenge that needs to be solved.

[0003] Solar phase change thermal storage materials directly capture and store solar energy through the phase change process. However, since the spectral absorption rate of the phase change material itself is usually low, the photothermal conversion efficiency is insufficient. To solve this problem, researchers have extensively explored methods of incorporating high-spectral absorption nanoparticles into phase change materials to improve their spectral absorption characteristics. These nanoparticles mainly include carbon nanoparticles, metal nanoparticles, and ceramic nanoparticles, which enhance the full-spectral absorption rate of phase change materials, thereby improving the efficiency of solar thermal storage.

[0004] Current research focuses on enhancing the full-spectrum absorption capacity of phase change materials by adding highly absorptive nanoparticles. However, there are relatively few studies on suppressing the infrared emissivity of phase change materials, especially in high-temperature applications. Infrared radiation loss under high temperature conditions is more significant, which will cause a large amount of heat loss and seriously affect the overall efficiency of solar phase change thermal storage. Therefore, while improving the full-spectrum absorption rate of phase change materials, suppressing infrared emissivity is also the key to improving the efficiency of solar thermal storage. Effectively solving this problem will have a profound impact on the application of solar phase change thermal storage materials under high temperature conditions. Summary of the invention

[0005] Purpose of the invention: The first purpose of the present invention is to provide a spectrally selective solar phase change heat storage material that can suppress the infrared emissivity of the phase change material; the second purpose of the present invention is to provide a method for preparing the spectrally selective solar phase change heat storage material.

[0006] Technical solution: The spectrally selective solar phase change heat storage material described in the present invention is composed of two layers of materials, the bottom layer is a porous silicon carbide material (porous silicon carbide ceramic skeleton) filled with phase change material, and the top layer is a plasma nanometal foil.

[0007] Combining porous silicon carbide filled with phase change material and plasma nanometal foil improves absorption efficiency across the solar spectrum At the same time, the infrared emissivity is suppressed This improves the efficiency of solar phase change thermal storage.

[0008] Preferably, the porosity of the porous silicon carbide material is 74-83%. Porosity plays a key role in the heat storage and release process of porous silicon carbide-based composite phase change materials. Lower porosity helps promote heat conduction, thereby increasing the heat transfer rate, but will lead to a decrease in energy storage density; higher porosity is conducive to increasing the load of the phase change material, thereby increasing the heat storage density, but will reduce the heat transfer rate. Experiments show that when the porosity of porous silicon carbide is 74% to 83%, the heat storage performance is optimal.

[0009] Preferably, the plasma nano-metal foil is a zinc foil loaded with copper nanoparticles.

[0010] Further preferably, the copper nanoparticles loaded on the zinc foil have a particle size of 60 to 70 nm. Changes in the size of copper nanoparticles will significantly affect the optical properties of the material, affecting its average spectral absorptivity and infrared emissivity. Research results show that when the particle size of the copper nanoparticles is 60 to 70 nm, the highest spectral absorptivity and lowest infrared emissivity can be obtained.

[0011] Preferably, the phase change material is dipentaerythritol. Other phase change materials can replace dipentaerythritol, such as all organic phase change materials, but the final calculated efficiency will vary due to different phase change materials.

[0012] Preferably, the porous silicon carbide ceramic skeleton is produced by impregnating graphite carbon felt with phenolic resin, carbonizing the carbonized carbon felt, and reacting the carbonized carbon felt with silicon. By using graphite carbon felt-phenolic resin as a precursor to prepare the silicon carbide skeleton, the porosity of the material can be flexibly controlled.

[0013] The method for preparing the spectrally selective solar phase-change heat storage material of the present invention comprises the following steps:

[0014] (1) Filling the porous silicon carbide material with a phase change material;

[0015] (2) The plasma nanometal foil is stacked on the upper surface of the porous silicon carbide material filled with phase change material.

[0016] Preferably, the preparation method of the porous silicon carbide material filled with phase change material is:

[0017] Ⅰ. The graphite carbon felt is cleaned and dried, then immersed in a phenolic resin solution, and then carbonized;

[0018] II. Taking sufficient amount of silicon powder and reacting with the carbonized graphite carbon felt in step I to generate silicon carbide; removing excess silicon to obtain a porous silicon carbide ceramic skeleton derived from the graphite carbon felt;

[0019] III. Using a vacuum impregnation method, dipentaquaternary alcohol is filled into the pores of the porous silicon carbide ceramic skeleton obtained in step II, thereby obtaining a graphite carbon felt-derived porous silicon carbide ceramic-based composite phase change material.

[0020] Preferably, the method for cleaning the graphite carbon felt is: cleaning the graphite carbon felt with ethanol and deionized water in sequence.

[0021] Preferably, the phenolic resin solution is obtained by dissolving phenolic resin in an ethanol solution and mechanically stirring the solution to obtain a uniform solution.

[0022] Preferably, the solid content of the phenolic resin solution is 60-70wt%. By adjusting the concentration of the phenolic resin used to impregnate the graphite carbon felt, porous silicon carbide materials with different porosities can be obtained. Experiments show that when the solid content of the phenolic resin is controlled at 60% to 70%, the optimal porosity (74% to 83%) can be obtained.

[0023] Preferably, in step I, the carbonization process is carried out in a tubular furnace, and the process parameters of the carbonization process are: the atmosphere is argon, the heating rate is 1-3°C / min, the carbonization temperature is 900-1100°C, and the insulation time is 0.5-1 hour.

[0024] Preferably, in step II, the carbonized graphite carbon felt reacts to generate silicon carbide by: taking a sufficient amount of silicon powder and the carbonized graphite carbon felt and placing them in a vacuum environment at a temperature of 1550-1600°C to react for 1.5-2 hours to generate silicon carbide; and sintering at a temperature of 1800°C-1850 for 2 hours, repeating the process to remove excess silicon to obtain a graphite carbon felt-derived porous silicon carbide skeleton.

[0025] Preferably, in step III, the vacuum impregnation method is: placing the porous ceramic skeleton and the dipentaerythritol phase change material in a tube furnace, heating to 230°C to 250°C, and keeping warm for 1.5 to 2 hours in a vacuum atmosphere to allow the dipentaerythritol to fill the pores of the porous silicon carbide ceramic skeleton.

[0026] Preferably, the plasma nanometal foil is a zinc foil loaded with copper nanoparticles, and the preparation method is as follows: the zinc foil is washed and immersed in a copper ion solution to generate copper nanoparticles on the surface of the zinc foil. After the reaction is completed, the zinc foil is quickly placed in deionized water to terminate the chemical reaction, and after drying, a spectrally selective solar energy absorbing plasma nanometal foil is obtained; in the replacement reaction, Cu 2+ The concentration is 0.012M~0.016M, the reaction temperature is 25℃~60℃, and the time is 30~45 seconds.

[0027] Preferably, the zinc foil is cleaned by placing the zinc foil in sulfuric acid solution, deionized water, acetone solution and deionized water in sequence for ultrasonic cleaning, and the process parameters are: the zinc foil is ultrasonically cleaned in a 2-2.5wt% sulfuric acid solution for 20-30 seconds, and cleaned in acetone or ethanol for 5-10 minutes.

[0028] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) By combining the porous silicon carbide material filled with phase change material and the plasma nanometal foil, the absorption efficiency in the solar spectrum range is improved, while the infrared radiation loss is suppressed; (2) The graphite carbon felt-derived silicon carbide skeleton provides good thermal conductivity, ensuring the effective transfer and storage of heat; (3) Dipentaerythritol is filled in the porous silicon carbide ceramic skeleton as a phase change material, providing excellent phase change heat storage performance, and can efficiently store and release thermal energy during temperature changes; (4) Copper nanoparticles are loaded on the zinc foil as a plasma nanometal foil, which increases the spectral selective absorption characteristics of the material, especially the suppression performance in the infrared band, and has a high spectral absorptivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a schematic diagram of the preparation process of the spectrally selective solar phase-change thermal storage material of the present invention;

[0030] Figure 2 The schematic diagram of the structure of the spectrally selective solar phase change thermal storage material in Example 2, wherein the material includes a graphite carbon felt-derived silicon carbide skeleton, dipentaerythritol, and plasma nanometal foil;

[0031] Figure 3 The schematic diagram of the structure of the spectrally selective solar phase change thermal storage material without plasma nanometal foil in Comparative Example 1 includes a graphite carbon felt-derived silicon carbide skeleton and di-tetrapentanol;

[0032] Figure 4 Schematic diagram of the preparation process of plasma nanometal foil;

[0033] Figure 5 The copper nanoparticle structure morphology of Examples 2, 3, and 4;

[0034] Figure 6 is the thermal conductivity diagram of Examples 1 to 2;

[0035] Figure 7 Enthalpy value test result diagram of comparative examples 1 to 2;

[0036] Figure 8 It is a spectrum comparison diagram of Examples 2, 3, and 4;

[0037] Fig. 9Spectral comparison diagram of Example 2, Comparative Example 1 and Comparative Example 2;

[0038] Fig.10 It is a comparison chart of the temperature rise curves of Example 2 and Comparative Example 1 under sunlight irradiation. DETAILED DESCRIPTION

[0039] The technical solution of the present invention is further described below in conjunction with embodiments.

[0040] Example 1

[0041] The preparation of the spectrally selective solar phase-change heat storage material of the present invention comprises the following steps:

[0042] 1. Preparation of porous silicon carbide ceramics derived from graphite carbon felt:

[0043] (1) washing the graphite carbon felt with ethanol and deionized water in turn and drying;

[0044] (2) dissolving a phenolic resin in an ethanol solution and mechanically stirring the solution to obtain a phenolic resin solution having a solid content of 60%;

[0045] (3) impregnating the graphite carbon felt in a phenolic resin solution so that its pores are filled with phenolic resin, and then placing it in a tubular furnace for carbonization. The process parameters of the carbonization process are: atmosphere is argon, heating rate is 1°C / min, carbonization temperature is 900°C, and holding time is 0.5 hour;

[0046] (4) taking a sufficient amount of silicon powder and the graphite carbon felt treated in step (3) and placing them in a vacuum environment, reacting at 1600° C. for 1.5 hours to generate silicon carbide, and sintering at 1800° C. for 2 hours. The process is repeated 3 times to remove excess silicon and obtain a porous silicon carbide skeleton derived from graphite carbon felt.

[0047] 2. Preparation of porous silicon carbide ceramic-based composite phase change materials derived from graphite carbon felt:

[0048] (1) placing the graphite carbon felt-derived porous silicon carbide skeleton and the diquaternary tetrapentanol phase change material obtained in step 1 above in a tube furnace;

[0049] (2) A vacuum impregnation method is used to fill dipentaquaternary alcohol into the pores of a porous silicon carbide ceramic skeleton, thereby obtaining a graphite carbon felt-derived porous silicon carbide ceramic-based composite phase change material; the process parameters are as follows: the porous silicon carbide ceramic and dipentaquaternary alcohol are placed in a tubular furnace, the temperature is raised to 250° C., and the temperature is kept in a vacuum atmosphere for 2 hours.

[0050] 3. Preparation of plasma nanometal foil:

[0051] (1) placing the zinc foil in a sulfuric acid solution, deionized water, an acetone solution, and deionized water for ultrasonic cleaning in sequence, wherein the process parameters are: the zinc foil is ultrasonically cleaned in a 2.5% sulfuric acid solution for 30 seconds and in an acetone solution for 5 minutes;

[0052] (2) immersing the cleaned zinc foil in a copper sulfate solution to generate a replacement reaction and generate copper nanoparticles on the surface of the zinc foil. The concentration of the copper sulfate solution is 0.016 M, the reaction temperature is 60° C., and the reaction time is 30 seconds.

[0053] (3) After the reaction is completed, the zinc foil is quickly placed in deionized water to terminate the chemical reaction, and after drying, a spectrally selective solar energy absorption material is obtained;

[0054] (4) Placing the plasma nanometal foil on the top surface of the graphite carbon felt-derived porous silicon carbide ceramic-based composite phase change material prepared in the above step 2 to obtain the spectrally selective solar thermal storage material named SiC / PCMs / PNC.

[0055] Example 2

[0056] On the basis of Example 1, in step 1, the solid content of the phenolic resin is changed to 70 wt %, and the other conditions remain unchanged.

[0057] Example 3

[0058] On the basis of Example 2, in step 3, the reaction temperature of the copper sulfate solution and the zinc sheet was changed to 20° C., and the other conditions remained unchanged.

[0059] Example 4

[0060] On the basis of Example 2, in step 3, the reaction temperature of the copper sulfate solution and the zinc sheet is changed to 40° C., and the other conditions remain unchanged.

[0061] Comparative Example 1

[0062] On the basis of Example 2, step 3 is omitted and other conditions remain unchanged, and the obtained product is named SiC / PCMs.

[0063] Comparative Example 2

[0064] Dipentaerythritol phase change materials (PCMs) were used without any other spectral enhancement or thermal conductivity enhancement treatment.

[0065] Comparative Example 3

[0066] On the basis of Example 2, step 1 and step 2 are not performed, and the pure phase change material dipentaerythritol is compounded with the plasma nano metal foil of step 3.

[0067] 1. Characterization of copper nanoparticle morphology

[0068] The morphology of the copper nanoparticles in Examples 2, 3, and 4 was characterized by a field emission scanning electron microscope (GeminiSEM 300) equipped with a backscattered electron detector. Figure 5 shown.

[0069] Depend on Figure 5 It can be seen that, compared with Examples 2, 3, and 4, when the reaction temperature increases from 20° C. to 60° C., the average diameter of the copper nanoparticles increases from about 30 nanometers to about 70 nanometers.

[0070] 2. Thermal conductivity test

[0071] The thermal conductivity of Examples 1 to 2 was tested, and the thermal diffusion coefficient of the samples was measured by laser flash analysis (Laser Flash Analysis, Linseis, LFA500). The results are as follows: Figure 6 shown.

[0072] The calculation formula for thermal diffusivity is α=ωL 2 / πt 1 / 2 , where α is the thermal diffusivity, L is the sample thickness, ω is a constant determined by the Clarke and Taylor approximation, and t 1 / 2 It is the time required for the back of the sample to reach half of its maximum temperature. Combined with the density ρ(T) of porous silicon carbide ceramics, the porosity of the sample can be determined by measuring the weight and volume of the sample. The calculation formula is P(%) = (1-ρ1 / ρ SiC )·100%, where ρ1 is the density of the prepared porous silicon carbide sample, ρ SiC is the density of dense silicon carbide. Specific heat capacity C p (T) can be obtained by differential scanning calorimetry DSC measurement. From this, the thermal conductivity of the material can be calculated:

[0073] k(T)=α(T)·C p (T)·ρ(T) (1)

[0074] The calculation shows that the porosity of the porous materials prepared in Examples 1 and 2 is 83% and 74% respectively. When the porosity is 74%, the thermal conductivity is 14.0 W m -1 K -1 When the porosity is 83%, the thermal conductivity is 3.7 W m -1 K -1 .

[0075] 3. Phase change enthalpy test:

[0076] The phase change enthalpy values ​​of Examples 1 to 2 were tested. The specific heat capacity and phase change enthalpy of the samples were tested based on differential scanning calorimetry (TA, Differential Scanning Calorimetry, DSC 25).

[0077] Figure 7 The DSC enthalpy test results of the PCMs of Comparative Example 2 and the SiC / PCMs composite material of Comparative Example 1 show that the melting peak temperature of PCMs is 224.28°C, and the corresponding enthalpy change is 374.00 kJ kg -1 ; Its solidification peak temperature is 200.99℃, and the corresponding enthalpy change is 370.94kJ kg -1 After being compounded with silicon carbide, the enthalpy values ​​of the melting and solidification processes of SiC / PCMs are 195.10 kJ kg -1 and 176.60 kJ kg -1 The enthalpy values ​​of the SiC / PCMs composite materials in Examples 2 to 4 are the same as the enthalpy value of the SiC / PCMs composite material in Comparative Example 1, and the enthalpy value has nothing to do with the plasma metal foil.

[0078] 4. Spectral characteristics test:

[0079] The spectral characteristics of Examples 2 to 4, Comparative Example 1, and Comparative Example 2 were tested. The solar spectrum absorption characteristics of the samples were measured using a UV-Vis-NIR Spectrophotometer (LAMBDA1050+). Under normal incidence conditions, the spectral absorption rate of the composite material in the wavelength range of 0.2 μm to 16 μm was measured. The test results are as follows: Figure 8 and 9 shown.

[0080] Depend on Figure 8 It can be obtained that the average solar spectrum absorptivity of Examples 2 to 4 is 90.57%, 62.27%, and 85.29%, respectively, and the average infrared spectrum emissivity is 7.47%, 8.23%, and 8.02%, respectively. It can be seen that as the size of copper nanoparticles increases from 30nm to 70nm, the solar spectrum absorptivity gradually increases. This shows that the reaction temperature has an important influence on the size of copper nanoparticles and the corresponding optical properties.

[0081] from Fig. 9It can be seen that there are significant differences in the spectral characteristics of Example 2 and Comparative Examples 1 and 2. For Comparative Example 2, the average solar spectrum absorptivity of the pure phase change material is only 9.41%, and the infrared emissivity is 67.7%. The absorptivity is low, and it is difficult to achieve effective solar energy capture. For Comparative Example 1, after the phase change material is compounded with silicon carbide, the average solar spectrum absorptivity of the SiC / PCMs composite material is significantly increased to 91.22%. This significant enhancement in absorptivity is mainly attributed to the multiple light scattering effect within the porous structure of silicon carbide; however, the infrared emissivity of the composite material is relatively high, at 71.94%, which will cause a large amount of infrared radiation loss at high temperatures. In Example 2, the SiC / PCMs composite material is further compounded with a plasma nanostructure to form a SiC / PCMs / PNC composite material, whose solar spectrum absorptivity is 90.57%, which is comparable to that of the SiC / PCMs composite material, and its infrared emissivity is significantly reduced to only 7.47%. By maintaining similar solar spectrum absorptivity of SiC / PCMs / PNC and SiC / PCMs composites, the effect of significantly reducing infrared emissivity on improving thermal storage efficiency is verified.

[0082] 5. Heat storage efficiency test

[0083] The temperature rise of Example 2 and Comparative Example 1 under direct sunlight was tested.

[0084] Test method: When the solar radiation intensity is 20kW·m -2 The solar thermal storage efficiency of solar thermal storage materials SiC / PCMs / PNC and SiC / PCMs materials containing plasma nanometal foil was tested after 240 seconds of solar radiation. The calculation formula for solar thermal storage efficiency is:

[0085]

[0086] Where η c is the solar thermal conversion efficiency; η s is the thermal energy storage efficiency, which depends on the thermal conductivity of the phase change thermal storage material; m is the mass of the phase change thermal storage material; ΔH is the latent heat of the phase change thermal storage material; P is the solar radiation intensity; Δt is the duration of the phase change process. The test results are as follows Fig.10 shown.

[0087] Depend on Fig.10It can be seen that under the same lighting conditions, the peak temperature of the material SiC / PCMs / PNC of Example 2 reached 251.68°C. In contrast, the maximum temperature of the material SiC / PCMs of Comparative Example 1 under the same irradiation conditions was 228.42°C, and the temperature difference between the two was 23.26°C. In addition, the experiment observed that the solar heat storage time of SiC / PCMs / PNC was only 48 seconds, which was significantly less than the 72 seconds of SiC / PCMs without infrared suppression function, and the heat storage time was shortened by about 1.5 times. Calculated by formula (2), the solar energy storage efficiency of the material SiC / PCMs / PNC of Example 2 was 81.65%, which was significantly better than the 54.56% of the material SiC / PCMs of Comparative Example 1. These results show that the solar energy storage efficiency of composite phase change materials can be significantly improved by suppressing infrared radiation losses.

Claims

1. A spectrally selective solar phase change thermal storage material, characterized in that: The material consists of two layers of materials, a bottom layer is a porous silicon carbide material filled with phase change material, and a top layer is a plasma nano metal foil.

2. The spectrally selective solar phase change thermal storage material according to claim 1, characterized in that: The porosity of the porous silicon carbide material is 74-83%.

3. The spectrally selective solar phase change thermal storage material according to claim 1, characterized in that: The plasma nano metal foil is a zinc foil loaded with copper nano particles.

4. The spectrally selective solar phase change thermal storage material according to claim 1, characterized in that: A layer of copper nanoparticles is loaded on the zinc foil, and the particle size of the copper nanoparticles is 60-70 nm.

5. The spectrally selective solar phase change thermal storage material according to claim 1, characterized in that: The phase change material is dipentaerythritol.

6. A method for preparing the spectrally selective solar phase-change thermal storage material according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) Filling the porous silicon carbide material with a phase change material; (2) The plasma nanometal foil is stacked on the upper surface of the porous silicon carbide material filled with phase change material.

7. The method for preparing the spectrally selective solar phase-change thermal storage material according to claim 6, characterized in that: The preparation method of the porous silicon carbide material filled with phase change material is: Ⅰ. The graphite carbon felt is cleaned and dried, then immersed in a phenolic resin solution, and then carbonized; II. Reaction of silicon powder with the carbonized graphite carbon felt in step I to generate silicon carbide, and removal of excess silicon to obtain a porous silicon carbide ceramic skeleton derived from the graphite carbon felt; III. Using vacuum impregnation method, dipentaquaternary alcohol is filled into the pores of the porous silicon carbide ceramic skeleton obtained in step II, so as to obtain a graphite carbon felt-derived porous silicon carbide ceramic-based composite phase change material.

8. The method for preparing the spectrally selective solar phase-change thermal storage material according to claim 6, characterized in that: The concentration of the phenolic resin solution is 60-70%.

9. The method for preparing the spectrally selective solar phase-change thermal storage material according to claim 6, characterized in that: The plasma nano metal foil is a zinc foil loaded with copper nano particles, and the preparation method is: the zinc foil is washed and immersed in a copper ion solution, copper nano particles are generated on the surface of the zinc foil through a replacement reaction, and the plasma nano metal foil with spectrally selective solar energy absorption material is obtained.

10. The method for preparing the spectrally selective solar phase-change thermal storage material according to claim 9, characterized in that: The replacement reaction conditions are: Cu 2+ The concentration is 0.012-0.016M, the reaction temperature is 25-60°C, and the reaction time is 30-45 seconds.

Citation Information

Patent Citations

  • Loofah-derived porous silicon carbide ceramic-based high-temperature photo-thermal storage material and preparation method thereof

    CN113800945A

  • Salinity difference cycle power generation system and method based on phase change material and solar photo-thermal

    CN114562433A

  • Sugarcane derived porous silicon carbide ceramic-based heat storage material, preparation method and device

    CN116376519A

  • Environment-friendly SiC heat storage material with PVC as raw material and preparation method of environment-friendly SiC heat storage material

    CN116751063A

  • Fluid discharge method for fluid leak response training

    KR102387671B1