Water-based diamond wire silicon wafer cutting fluid and preparation method thereof
By improving the composition of the diamond wire cutting fluid, a lubricating film and improved permeability were formed, solving the problems of insufficient lubrication and permeability, and improving the efficiency and stability of silicon wafer cutting.
Patent Information
- Application Number
- CN202411098375.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-29
AI Technical Summary
Existing diamond wire cutting fluids have insufficient lubrication, penetration, and emulsification properties, resulting in low efficiency in cutting silicon wafers.
A combination of components such as polyether, lubricant, penetrant, and emulsifier is used to form a lubricating film, which reduces the coefficient of friction, improves permeability and emulsification, and ensures that all components of the cutting fluid are uniformly suspended, avoiding stratification.
It improves the efficiency of silicon wafer cutting, reduces the coefficient of friction and mechanical damage on the silicon wafer surface, and enhances the stability and service life of the cutting fluid.
Smart Images

Figure CN119040056A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of solar cells, and in particular relates to an aqueous diamond wire silicon wafer cutting fluid and a preparation method thereof. Background Art
[0002] Solar cell power generation is a sustainable source of clean energy. It uses the photovoltaic effect of semiconductor pn junction to convert sunlight into electrical energy. Silicon wafers are the basic materials for preparing solar cells. Silicon wafer cutting is a very important link in the photovoltaic industry chain. The quality of silicon wafer cutting directly affects the downstream battery production. Diamond wire cutting technology is the mainstream silicon wafer cutting technology in the existing technology. In diamond wire cutting technology, the hardness and sharp edges of diamond particles are fully utilized to gradually saw off silicon rods. This process is accompanied by large friction heat. Therefore, diamond-specific wire cutting fluid must have good lubrication and penetration properties.
[0003] For example, patent document CN106939182A discloses an aqueous diamond wire silicon wafer cutting fluid and a method for making the same, comprising the following weight portions: polyether: 10% to 35%, dispersing wetting agent 12% to 25%, penetrant 3% to 5%, antirust and antibacterial agent 0.1% to 0.2% and defoamer 1% to 4%, wherein the dispersing wetting agent comprises polyethylene glycol, and the penetrant is fatty alcohol polyoxyethylene ether. However, there are disadvantages in using polyethylene glycol as a dispersing wetting agent in silicon wafer cutting fluid. Specifically, the hygroscopicity and thermal oxidation properties of polyethylene glycol are factors affecting the instability during wire cutting. In addition, fatty alcohol polyoxyethylene ether as a dispersing wetting agent cannot provide satisfactory penetration performance.
[0004] How to continuously improve diamond wire cutting technology and increase the efficiency of cutting silicon wafers is an urgent problem to be solved in diamond wire cutting technology. Summary of the invention
[0005] The present application provides a water-based diamond wire silicon wafer cutting fluid formula, which aims to improve the lubrication performance, penetration performance and emulsification performance of the diamond wire silicon wafer cutting fluid formula in the prior art, improve the performance of the cutting fluid and thereby improve the efficiency of cutting silicon wafers.
[0006] According to a first aspect of the present invention, an embodiment of the present application provides an aqueous diamond wire silicon wafer cutting fluid, comprising the following components by weight:
[0007] 20% to 50% of a dispersant selected from polyether;
[0008] 5% to 15% lubricant;
[0009] 2% to 10% penetrant;
[0010] 1% to 10% emulsifier; and the balance is water.
[0011] Furthermore, the polyether is selected from one or more of C4 alcohol mono-terminated ethylene oxide / propylene oxide block copolyethers and C6 alcohol mono-terminated ethylene oxide / propylene oxide block copolyethers.
[0012] Furthermore, the lubricant is selected from dodecylbenzene.
[0013] Furthermore, the penetrant is selected from secondary alcohol polyoxyethylene ether.
[0014] Furthermore, the emulsifier is selected from long-chain carboxylic acid ester polyoxyethylene-18.
[0015] Furthermore, the aqueous diamond wire silicon wafer cutting fluid further comprises the following components by weight:
[0016] 0.2% to 0.6% of a chelating agent, selected from one or more of disodium EDTA, sodium citrate, and sodium gluconate;
[0017] 0.1% to 0.2% of an antibacterial agent selected from sodium molybdate;
[0018] 0.1% to 0.2% of rust inhibitor, selected from one or more of MC tribasic acid, sebacic acid, and dodecanedioic acid;
[0019] 3% to 5% of a defoaming agent selected from silicone amide; and
[0020] 1% to 3% of a pH regulator is selected from malonic acid.
[0021] Furthermore, the aqueous diamond wire silicon wafer cutting fluid comprises the following components by weight:
[0022] 30% to 38% dispersant;
[0023] 7% to 11% lubricant;
[0024] 4% to 8% penetrant;
[0025] 3% to 7% emulsifier; and the balance is water.
[0026] According to a second aspect of the present invention, an embodiment of the present application provides a method for preparing an aqueous diamond wire silicon wafer cutting fluid, comprising the following steps:
[0027] S1. Mix the dispersant, lubricant, penetrant, emulsifier and the balance of water and stir for 10 to 20 minutes to form a first mixture;
[0028] S2. Adding a chelating agent, an antibacterial agent, a rust inhibitor, a defoaming agent and a pH regulator to the first mixture, and continuing stirring for 100 min to 170 min;
[0029] S3. The solution at the bottom layer is pumped to the upper layer and circulated for 5 to 20 minutes to obtain a silicon wafer cutting solution;
[0030] Wherein, the polyether, the lubricant, the emulsifier, the antibacterial agent, the rust inhibitor, the defoaming agent and the pH adjuster are according to the present invention.
[0031] The lubricant in the cutting fluid according to the present invention can form a lubricating film between the diamond wire and the silicon wafer, thereby reducing the friction coefficient of the silicon wafer surface. The penetrant in the cutting fluid can reduce the surface tension of the cutting fluid, so that the cutting fluid can easily penetrate between the diamond wire and the silicon wafer to reduce the mechanical damage to the silicon wafer. In addition, the emulsifier in the cutting fluid can make the various components in the cutting fluid more evenly suspended in the aqueous phase without stratification. Thanks to the mutual coordination of the various components in the cutting fluid, the performance of the cutting fluid is improved, thereby improving the efficiency of cutting silicon wafers. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a schematic diagram of the preparation method of the aqueous diamond wire silicon wafer cutting fluid in Example 4 of the present application. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0034] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.
[0035] Embodiment 1
[0036] This embodiment provides a formula for a water-based diamond wire silicon wafer cutting fluid, which specifically includes the following components by weight:
[0037] 35% C4 alcohol mono-terminated ethylene oxide / propylene oxide block copolyether as dispersant;
[0038] 9% dodecylbenzene as lubricant;
[0039] 6% secondary alcohol polyoxyethylene ether as penetrant;
[0040] 5% long-chain carboxylic acid ester polyoxyethylene-18 as emulsifier;
[0041] 0.15% sodium molybdate as an antibacterial agent;
[0042] 0.15% ternary polycarboxylic acid as a rust inhibitor;
[0043] 4% silicone amide as defoamer;
[0044] 0.5% of malonic acid served as a pH adjuster; and the balance was water.
[0045] The dispersant in the cutting fluid can adsorb on the surface of the particles to generate a potential barrier, which can hinder the agglomeration of particles, and can generate entropy repulsion and osmotic hydration force to reduce the strength between the microcracks of the particle clusters, thus facilitating the cracking of the particle clusters. Using C4 alcohol mono-terminated ethylene oxide / propylene oxide block copolyether as a dispersant can particularly improve the dispersibility of the cutting fluid. In this field, the so-called "C4 alcohol" refers to an alcohol with four carbon groups. C4 alcohol mono-terminated ethylene oxide / propylene oxide block copolyether has the functions of dispersing, washing, defoaming, wetting, etc., and is relatively low in price, making it an ideal dispersant component.
[0046] Lubricants can lubricate the surface of an object and reduce the coefficient of friction. Dodecylbenzene, as a lubricant, can improve the hygroscopicity and thermal oxidation properties of cutting fluids. Dodecylbenzene lacks polar functional groups in its structure, so the polarity of the molecule is low. Due to its low polarity chemical structure, dodecylbenzene is not easy to react with oxygen under normal chemical conditions.
[0047] The penetrant can penetrate into the cracks at the front of the cutting area to form chemical energy splitting, which is beneficial to improving the cutting efficiency.
[0048] Emulsifiers have the function of reducing surface tension. Long-chain carboxylic acid ester polyoxyethylene-18, also known as LMEO-18, is a new type of non-ionic surfactant. In cutting fluid, long-chain carboxylic acid ester polyoxyethylene-18 can improve the emulsification effect, which will be explained in detail below.
[0049] Chelating agents can form complexes with metal ions, allowing them to stably exist in the cutting fluid, which helps prevent oxidation and precipitation of metal ions, reduce the impurity content in the cutting fluid, and improve the stability and service life of the cutting fluid.
[0050] Antibacterial agents can prevent the growth of microorganisms in the cutting fluid and extend the shelf life of the cutting fluid.
[0051] Rust inhibitors can prevent the diamond wire used to cut silicon wafers from rusting.
[0052] Defoamers prevent bubbles from forming during the cutting process.
[0053] The pH adjuster is used to adjust the pH value of the cutting fluid, which is generally between 5 and 7.
[0054] As a comparison, a comparative example 1 is set up, in which the lubricant in the above formula is replaced with polyethylene glycol in the prior art, and the other components remain unchanged. The performance of the cutting fluid formula is evaluated by measuring the cutting torque, silicon wafer line mark value and total thickness deviation (TTV) during the cutting process. The measurement results are shown in Table 1 below.
[0055] The test process of average cutting torque is as follows: when cutting 820mm long silicon rods with a high-precision slicer, the slicer displays the maximum cutting torque (unit: N·m). n silicon rods are cut once with the same cutting fluid, and the average cutting torque is calculated.
[0056] The test process of the average line mark value and the maximum TTV value is as follows: after sorting the same type of silicon wafers with the Autevi silicon wafer sorter, record the average line mark value and the maximum TTV value, use the same cutting fluid formula to cut n silicon rods once to obtain three silicon wafer samples and calculate their average values.
[0057]
[0058]
[0059] Table 1. Cutting fluid components and performance test results of Example 1 and Comparative Example 1
[0060] As can be seen from Table 1, compared with Comparative Example 1, Example 1 has fewer cutting knives, lower average cutting torque, lower line mark average value and lower TTV maximum value. Thanks to the fact that dodecylbenzene in Example 1 can form a lubricating film between the diamond wire and the silicon wafer as a lubricant, the friction coefficient on the surface of the silicon wafer is reduced. Dodecylbenzene as a lubricant can significantly improve the lubrication performance of the cutting fluid, and the smaller the friction coefficient on the silicon wafer surface, the smaller the cutting torque, the smaller the silicon wafer line mark value and the smaller the TTV. This is of great significance for cutting silicon wafers and the downstream production of solar cells, and can effectively improve production efficiency.
[0061] Embodiment 2
[0062] This embodiment provides another water-based diamond wire silicon wafer cutting fluid formula, which specifically includes the following components by weight:
[0063] 30% C4 alcohol mono-terminated ethylene oxide / propylene oxide block copolyether as dispersant;
[0064] 11% dodecylbenzene as lubricant;
[0065] 6% secondary alcohol polyoxyethylene ether as penetrant;
[0066] 5% long-chain carboxylic acid ester polyoxyethylene-18 as emulsifier;
[0067] 0.2% sodium molybdate as an antibacterial agent;
[0068] 0.2% ternary polycarboxylic acid as rust inhibitor;
[0069] 5% silicone amide as defoamer;
[0070] 1% of malonic acid served as a pH adjuster; and the balance was water.
[0071] As a comparison, a comparative example 2 is set, in which the penetrant is replaced with a fatty alcohol polyoxyethylene ether in the prior art, and the other components remain unchanged. Similar to Example 1, the performance of the cutting fluid formula is evaluated by measuring the cutting torque, wire breakage rate, line mark average value and total thickness deviation (TTV) during the cutting process. The measurement results are shown in Table 2 below. The measuring method of the cutting torque, line mark average value and total thickness deviation (TTV) in this embodiment is the same as that recorded in Example 1.
[0072] The wire breakage rate is measured as follows: use a high-precision slicer with cutting fluid to cut n 820 mm long silicon rods, and record the number of silicon rods x that have been cut before the diamond wire breaks during the cutting process. The wire breakage rate is x / n×100%.
[0073]
[0074] Table 2. Cutting fluid components and performance test results of Example 2 and Comparative Example 2
[0075] As can be seen from Table 2, compared with Comparative Example 2, Example 2 has fewer cutting knives, lower wire breakage rate, smaller average wire mark value and smaller TTV. Thanks to the secondary alcohol polyoxyethylene ether in Example 2 as a penetrant, the surface tension of the cutting liquid can be reduced, so that the cutting liquid can easily penetrate between the diamond wire and the silicon wafer to reduce mechanical damage to the silicon wafer. Therefore, compared with Comparative Example 2, the cutting liquid in Example 2 containing long-chain carboxylic acid ester polyoxyethylene-18 as an emulsifier has better penetration performance, especially the lower wire breakage rate, which is of great significance for the production of silicon wafers and thus the production of solar cells.
[0076] Embodiment 3
[0077] This embodiment provides another water-based diamond wire silicon wafer cutting fluid formula, which specifically includes the following components by weight:
[0078] 40% C6 alcohol mono-terminated ethylene oxide / propylene oxide block copolyether as dispersant;
[0079] 9% dodecylbenzene as lubricant;
[0080] 6% secondary alcohol polyoxyethylene ether as penetrant;
[0081] 5% long-chain carboxylic acid ester polyoxyethylene-18 as emulsifier;
[0082] 0.2% sodium citrate as a chelating agent;
[0083] 0.15% sodium molybdate as an antibacterial agent;
[0084] 0.15% ternary polycarboxylic acid as a rust inhibitor;
[0085] 4% silicone amide as defoamer;
[0086] 0.5% of malonic acid served as a pH adjuster; and the balance was water.
[0087] After the cutting fluid was mixed and allowed to stand for 10 minutes, stratification was observed. The upper layer after stratification was measured with a ruler, and the measurement results are shown in Table 3 below.
[0088]
[0089]
[0090] Table 3. Cutting fluid components and performance test results of Example 3 and Comparative Example 3
[0091] The better the emulsification performance of the cutting fluid, the smaller the thickness of the upper layer after standing. From the results in Table 3, it can be seen that the thickness of the layer after standing of the cutting fluid formula containing 5% long-chain carboxylic acid ester polyoxyethylene-18 as an emulsifier (i.e., Example 3) is much lower than that of the cutting fluid formula without adding 5% long-chain carboxylic acid ester polyoxyethylene-18 (i.e., Comparative Example 3). Thanks to the long-chain carboxylic acid ester polyoxyethylene-18 as an emulsifier in the cutting fluid, the various components in the cutting fluid are more evenly suspended in the water phase without stratification.
[0092] Embodiment 4
[0093] This embodiment provides a method for preparing a silicon wafer cutting fluid, such as Figure 1 As shown, the following steps are included:
[0094] S1. 35% by weight of C4 alcohol mono-terminated ethylene oxide / propylene oxide block copolyether (dispersant), 9% of dodecylbenzene (lubricant), 6% of secondary alcohol polyoxyethylene ether (penetrant), 5% of long-chain carboxylic acid ester polyoxyethylene-18 (emulsifier) and the remainder of water are mixed and stirred for 10 to 20 minutes to form a first mixture;
[0095] S2. Add 0.4% by weight of disodium ethylenediaminetetraacetate (chelating agent), 0.15% of sodium molybdate (bacteriostatic agent), 0.15% of ternary polycarboxylic acid (rust inhibitor), 4% of silicone amide (defoaming agent) and 0.5% of malonic acid (pH regulator) to the first mixture, and continue stirring for 150 min;
[0096] S3. Use a water pump to pump the solution at the bottom layer to the upper layer and circulate it for 15 minutes to obtain the silicon wafer cutting liquid. This circulation can fully disperse the various components in the cutting liquid to avoid stratification.
[0097] Optionally, after step S3, the silicon wafer cutting fluid is inspected, qualified products are packaged, and unqualified products are treated as unqualified products.
[0098] In this embodiment, it can be understood that the selection and dosage of all components can be adjusted according to actual needs.
[0099] The lubricant in the cutting liquid according to the present invention can form a lubricating film between the diamond wire and the silicon wafer, thereby reducing the friction coefficient of the silicon wafer surface. The penetrant in the cutting liquid can reduce the surface tension of the cutting liquid, so that the cutting liquid can easily penetrate between the diamond wire and the silicon wafer to reduce the mechanical damage to the silicon wafer. In addition, the emulsifier in the cutting liquid can make the various components in the cutting liquid more evenly suspended in the aqueous phase without stratification. Thanks to the mutual coordination of the various components in the cutting liquid, the performance of the cutting liquid is improved, thereby improving the efficiency of cutting the silicon wafer.
[0100] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent replacements and improvements made within the spirit and principles of the present application shall be included in the protection scope of the present application. For example, the technical features described in one embodiment may be used in another embodiment to obtain a further embodiment.
Claims
1. A water-based diamond wire silicon wafer cutting fluid, characterized in that: It comprises the following components by weight: 20% to 50% of a dispersant selected from polyether; 5% to 15% lubricant; 2% to 10% penetrant; 1% to 10% emulsifier; and the balance is water.
2. The aqueous diamond wire silicon wafer cutting fluid according to claim 1, characterized in that: The polyether is selected from one or more of C4 alcohol mono-terminated ethylene oxide / propylene oxide block copolyethers and C6 alcohol mono-terminated ethylene oxide / propylene oxide block copolyethers.
3. The aqueous diamond wire silicon wafer cutting fluid according to claim 1, characterized in that: The lubricant is selected from dodecylbenzene.
4. The aqueous diamond wire silicon wafer cutting fluid according to claim 1, characterized in that: The penetrant is selected from secondary alcohol polyoxyethylene ether.
5. The aqueous diamond wire silicon wafer cutting fluid according to claim 1, characterized in that: The emulsifier is selected from long-chain carboxylic acid ester polyoxyethylene-18.
6. The aqueous diamond wire silicon wafer cutting fluid according to claim 1, characterized in that: Also includes the following components by weight: 0.2% to 0.6% of a chelating agent, selected from one or more of disodium EDTA, sodium citrate, and sodium gluconate; 0.1% to 0.2% of an antibacterial agent selected from sodium molybdate; 0.1% to 0.2% of rust inhibitor, selected from one or more of MC tribasic acid, sebacic acid, and dodecanedioic acid; 3% to 5% of a defoaming agent selected from silicone amide; and 1% to 3% of a pH regulator is selected from malonic acid.
7. The aqueous diamond wire silicon wafer cutting fluid according to claim 1, characterized in that: It comprises the following components by weight: 30% to 38% dispersant; 7% to 11% lubricant; 4% to 8% penetrant; 3% to 7% emulsifier; and the balance is water.
8. A method for preparing an aqueous diamond wire silicon wafer cutting fluid, characterized in that: The following steps are involved: S1. Mix the dispersant, lubricant, penetrant, emulsifier and the balance of water and stir for 10 to 20 minutes to form a first mixture; S2. Adding a chelating agent, an antibacterial agent, a rust inhibitor, a defoaming agent and a pH regulator to the first mixture, and continuing stirring for 100 min to 170 min; S3. The solution at the bottom layer is pumped to the upper layer and circulated for 5 to 20 minutes to obtain a silicon wafer cutting solution; Wherein, the polyether, the lubricant, the emulsifier, the antibacterial agent, the rust inhibitor, the defoaming agent and the pH adjuster are as described in any one of claims 1 to 7.
Citation Information
Patent Citations