Ultralow-adsorption surface coating treatment scheme
Through the steps of pretreatment, plasma cleaning, superhydrophilic treatment and anti-protein adsorption substance coating, the problem of the deterioration of ultra-low adsorption characteristics of culture vessels during long-term use is solved, and the stability of the surface of the culture vessel and the accuracy of experimental results are achieved. It is suitable for a variety of cell culture needs, reducing experimental costs.
Patent Information
- Application Number
- CN202411173643.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing super-hydrophilic culture vessels are difficult to maintain ultra-low adsorption characteristics during long-term use, and are prone to adsorb biomolecules and contaminants, which affects the accuracy and repetition of experimental results, and cannot effectively maintain surface characteristics under complex biological conditions. .
Pretreatment, plasma cleaning, super hydrophilic treatment, enhanced modification treatment and drying steps, including ethanol and deionized water rinsing, plasma treatment, acrylic reagent steam treatment, anti-protein adsorption substance coating and drying, forming Stable ultra-low adsorption surface coating.
It realizes the stable and long-lasting ultra-low adsorption characteristics of the surface of the culture vessel, reduces biomolecular adsorption, improves the repeatability and accuracy of experimental results, and is suitable for a variety of cell culture methods, reducing experimental costs and resource consumption.
Smart Images

Figure CN119040124A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of surface coating treatment, and in particular to an ultra-low adsorption surface coating treatment scheme. Background Art
[0002] Superhydrophilic technology is a new technology that changes the surface properties of materials. The surface of the material treated with this technology has important characteristics such as anti-adhesion, anti-fog, anti-pollution, self-cleaning and prevention of current conduction. It has broad application prospects in many fields such as scientific research, production, and life.
[0003] In the field of biology, the application of superhydrophilic and ultra-low adhesion technologies has brought significant advantages in cell culture and experiments, especially in cell suspension culture, tumor spheroid culture and embryoid body formation experiments. However, the culture vessels that have undergone initial superhydrophilic treatment have the problem of not being able to maintain ultra-low adsorption properties for a long time, which mainly includes the following disadvantages:
[0004] 1. Surface treatment durability issues: Culture vessels that have been treated with initial super-hydrophilicity usually have good ultra-low adsorption properties at the beginning, but these properties will gradually weaken or fail over time. The surface of the culture vessel may be affected by the culture conditions and operation process, resulting in the performance degradation of the super-hydrophilic material or coating;
[0005] 2. Biological attachment and contamination: In practical applications, the surface of culture vessels is easily adsorbed by biological molecules, cell fragments or other contaminants, which may change the super-hydrophilic properties of the surface or increase its surface adhesion. Biological attachment and contamination will not only affect the ultra-low adhesion performance of the culture vessel, but also may affect the accuracy and repeatability of the experimental results.
[0006] 3. Meeting the challenges of complex biological conditions: Under complex biological conditions, such as long-term culture, multiple operations, and culture of specific cell types, culture vessels treated with super-hydrophilicity may not be able to effectively maintain their ultra-low adsorption properties. Specific cell types or culture conditions may require more stringent surface treatment and design to meet higher challenges and requirements.
[0007] Therefore, it is necessary to design an ultra-low adsorption surface coating treatment solution to solve the above problems. Summary of the invention
[0008] The purpose of the present invention is to solve the shortcomings of the prior art and to propose an ultra-low adsorption surface coating treatment solution.
[0009] In order to achieve the above object, the present invention adopts the following technical solutions:
[0010] An ultra-low adsorption surface coating treatment scheme comprises the following steps:
[0011] Step 1: Pretreatment: Perform preliminary cleaning on the medical materials to be treated to confirm the surface dirtiness. Non-sterile products need to be rinsed with ethanol and deionized water first, then ultrasonically cleaned under ethanol conditions for half an hour, and rinsed with deionized water for half an hour. Finally, put the materials in an oven to dry for later use to ensure that the surface is dry.
[0012] Step 2: Plasma cleaning: Plasma cleaning is performed in an argon atmosphere to open the chemical bonds on the surface of the material and set the plasma treatment parameters;
[0013] Step 3: Super-hydrophilic treatment: Use acrylic acid reagent for super-hydrophilic treatment. Set the heating module to heat the argon gas to 110°C, and introduce the acrylic acid reagent to evaporate it and bring it into the plasma instrument in a vacuum environment. Control the reagent steam flow meter to ensure that the incoming gas flow is 20cm 3 / min, processing time is 10-15 minutes;
[0014] Step 4: Enhanced modification treatment: placing the surface treated with ultra-low adsorption modification in a solution of an anti-protein adsorption substance to evenly coat the surface;
[0015] Step 5: Drying and standby: Dry the processed materials for half an hour.
[0016] As a preferred technical solution of the present invention, in step 2, the plasma processing parameters are set as follows:
[0017] Power: 600W;
[0018] Oxygen intake volume: 200sccm;
[0019] Argon gas inlet volume: 50sccm;
[0020] Vacuum environment: 30Pa;
[0021] Processing time: 480 seconds.
[0022] As a preferred technical solution of the present invention, in step 4, the method of covering the surface with the solution includes:
[0023] Spraying method: Use a spray device to evenly spray the solution of the anti-protein adsorption substance on the surface;
[0024] Immersion method: completely immerse the treated material in a solution of anti-protein adsorption substances.
[0025] As a preferred technical solution of the present invention, in the step five, a drying oven is used as a drying device to ensure that the inside of the oven is clean, and the temperature and time are set. The oven temperature is set between 50°C and 60°C. This temperature range supports rapid drying of the material surface without destroying the chemical properties of the surface coating. The treated material is placed on an oven tray for 30 minutes to ensure that the surface coating of the material is completely dry and fixed. After drying, the material is allowed to cool naturally to room temperature in the oven to avoid moving or handling hot materials prematurely.
[0026] As a preferred technical solution of the present invention, in the step one, the medical material to be treated is preliminarily cleaned, the surface is checked for residues, and the surface of the material is cleaned with an appropriate detergent and a soft cloth to ensure the removal of visible stains and particulate matter. For non-sterile products, 75% ethanol is first used for rinsing, and the ethanol is covered on the surface of the material and left on the surface for 5-10 minutes. Under ethanol conditions, ultrasonic cleaning equipment is used for ultrasonic cleaning. Finally, the cleaned material is finally rinsed with deionized water.
[0027] The present invention has the following beneficial effects:
[0028] 1. Stable ultra-low adsorption characteristics: The use of pre-treatment technology and ultra-low adsorption reagent treatment can form a stable and lasting super-hydrophilic property on the surface of the cell culture container. This characteristic makes the cell culture container less susceptible to adsorption of biological molecules during long-term use, thereby maintaining the stability and consistency of the cell culture environment;
[0029] 2. Suitable for a variety of culture methods: The treated cell culture container is not only suitable for traditional adherent cell culture, but also supports cell suspension culture and special types of culture experiments, such as tumor spheroid culture and embryoid body formation experiments. This versatility allows the same cell culture container to meet the needs of different types of biological experiments;
[0030] 3. Improve the repeatability and accuracy of experimental results: The ultra-low adsorption characteristics of the cell culture container surface can significantly reduce the non-specific adsorption of biomolecules, help reduce the variability in the experiment, and improve the repeatability and accuracy of the experimental results, which is particularly important for basic research or drug screening.
[0031] 4. Enhance the stability of the cell growth environment: Cells are highly sensitive to the culture environment. By reducing the nonspecific adsorption on the surface of the culture container, the sensitivity to changes in the culture fluid components can be reduced, thereby enhancing the growth stability and health of cells;
[0032] 5. Reduce experimental costs: The long-term stable ultra-low adsorption characteristics mean that the frequency of replacement of cell culture containers is reduced, thereby reducing laboratory operating costs and resource consumption and improving experimental efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a flow chart of the steps of an ultra-low adsorption surface coating treatment solution proposed by the present invention. DETAILED DESCRIPTION
[0034] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0035] Reference Figure 1 , a surface coating treatment scheme with ultra-low adsorption, comprising the following steps:
[0036] Step 1, pretreatment: perform preliminary cleaning of the medical materials to be treated and confirm the surface dirtiness. Non-sterile products need to be rinsed with ethanol and deionized water first, then ultrasonically cleaned under ethanol conditions for half an hour, and rinsed with deionized water for half an hour. Finally, put the materials in an oven for drying and use, ensuring that the surface is dry. In step 1, perform preliminary cleaning of the medical materials to be treated, check whether there are any residues on the surface, use appropriate detergents and soft cloth to clean the surface of the materials, and ensure that visible stains and particles are removed. For non-sterile products, first rinse with 75% ethanol, cover the surface of the material with ethanol, and leave it on the surface for 5-10 minutes. Under ethanol conditions, use ultrasonic cleaning equipment for ultrasonic cleaning. Finally, use deionized water to rinse the cleaned materials for the final time;
[0037] Step 2, plasma cleaning: plasma cleaning is performed in an argon atmosphere to open the chemical bonds on the surface of the material and set the plasma processing parameters. In step 2, the plasma processing parameters set are: power: 600W; oxygen intake: 200sccm; argon intake: 50sccm; vacuum environment: 30Pa; processing time: 480 seconds;
[0038] Step 3: Super-hydrophilic treatment: Use acrylic acid reagent for super-hydrophilic treatment. Set the heating module to heat the argon gas to 110°C, and introduce the acrylic acid reagent to evaporate it and bring it into the plasma instrument in a vacuum environment. Control the reagent steam flow meter to ensure that the incoming gas flow is 20cm 3 / min, processing time is 10-15 minutes;
[0039] Step 4, enhanced modification treatment: placing the surface treated with ultra-low adsorption modification in a solution of an anti-protein adsorption substance to uniformly coat the surface. In step 4, the method of covering the surface with the solution includes: spraying method: using a spray device to uniformly spray the solution of the anti-protein adsorption substance on the surface; immersion method: completely immersing the treated material in the solution of the anti-protein adsorption substance;
[0040] Step 5, drying and standby: dry the treated materials for half an hour. In step 5, use a drying oven as the drying equipment, ensure that the inside of the oven is clean, and set the temperature and time. Set the oven temperature between 50°C and 60°C. This temperature range supports rapid drying of the material surface without destroying the chemical properties of the surface coating. Place the treated material on the oven tray for 30 minutes to ensure that the surface coating of the material is completely dry and fixed. After drying, wait for the material to cool naturally to room temperature in the oven to avoid moving or handling hot materials prematurely.
[0041] The specific working principle of the present invention is as follows:
[0042] First, in the pretreatment stage, the material undergoes preliminary cleaning and ethanol rinsing to remove stains and particles on the surface. Next, in the plasma cleaning stage, argon plasma treatment is used to open the chemical bonds on the material surface and enhance the surface activity and receptivity. Subsequently, in the superhydrophilic treatment stage, acrylic reagents are used to make the material surface more hydrophilic through a plasma environment under heating and vacuum conditions, which is conducive to the use and application of biomaterials. In the following enhanced modification treatment stage, the surface is evenly coated with a solution of anti-protein adsorption substances by spraying or immersion to further enhance its anti-protein adsorption performance. Finally, after drying and curing treatment, the coating is ensured to be completely dry and fixed to provide a long-term and stable surface modification effect. The entire process combines physical and chemical methods to provide optimized functionality and biocompatibility for the surface of medical materials to meet the high requirements of medical devices and biomedical applications.
[0043] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A surface coating treatment scheme with ultra-low adsorption, characterized in that: The following steps are involved: Step 1: Pretreatment: Perform preliminary cleaning on the medical materials to be treated to confirm the surface dirtiness. Non-sterile products need to be rinsed with ethanol and deionized water first, then ultrasonically cleaned under ethanol conditions for half an hour, and rinsed with deionized water for half an hour. Finally, put the materials in an oven to dry for later use to ensure that the surface is dry. Step 2: Plasma cleaning: Plasma cleaning is performed in an argon atmosphere to open the chemical bonds on the surface of the material and set the plasma treatment parameters; Step 3: Super-hydrophilic treatment: Use acrylic acid reagent for super-hydrophilic treatment. Set the heating module to heat the argon gas to 110°C, and introduce the acrylic acid reagent to evaporate it and bring it into the plasma instrument in a vacuum environment. Control the reagent steam flow meter to ensure that the incoming gas flow is 20cm 3 / min, processing time is 10-15 minutes; Step 4: Enhanced modification treatment: placing the surface treated with ultra-low adsorption modification in a solution of an anti-protein adsorption substance to evenly coat the surface; Step 5: Drying and standby: Dry the processed materials for half an hour.
2. The ultra-low adsorption surface coating treatment solution according to claim 1, characterized in that: In step 2, the plasma processing parameters are set as follows: Power: 600W; Oxygen intake volume: 200sccm; Argon gas inlet volume: 50sccm; Vacuum environment: 30Pa; Processing time: 480 seconds.
3. The ultra-low adsorption surface coating treatment solution according to claim 1, characterized in that: In the step 4, the method of covering the surface with the solution comprises: Spraying method: Use a spray device to evenly spray the solution of the anti-protein adsorption substance on the surface; Immersion method: completely immerse the treated material in a solution of anti-protein adsorption substances.
4. The ultra-low adsorption surface coating treatment solution according to claim 1, characterized in that: In step five, a drying oven is used as the drying equipment, the inside of the oven is ensured to be clean, and the temperature and time are set. The oven temperature is set between 50°C and 60°C. This temperature range supports rapid drying of the material surface without destroying the chemical properties of the surface coating. The treated material is placed on the oven tray for 30 minutes to ensure that the surface coating of the material is completely dry and fixed. After drying, the material is allowed to cool naturally to room temperature in the oven to avoid moving or handling hot materials prematurely.
5. The ultra-low adsorption surface coating treatment solution according to claim 1, characterized in that: In the step 1, the medical materials to be treated are preliminarily cleaned, and the surface is checked for residues. The surface of the material is cleaned with an appropriate cleaning agent and a soft cloth to ensure that visible stains and particles are removed. For non-sterile products, 75% ethanol is first used for rinsing. The ethanol is covered on the surface of the material and left on the surface for 5-10 minutes. Under ethanol conditions, ultrasonic cleaning equipment is used for ultrasonic cleaning. Finally, the cleaned material is finally rinsed with deionized water.