Smelting method of ultrahigh-nitrogen ultralow-carbon Fe-Cr-Ni-based high-temperature alloy
Through the process route of electric furnace + AOD furnace + LF furnace + electroslag, combined with the reduction reaction of aluminum and ferrosilicon, oxygen blowing and nitrogen blowing, as well as the use of deoxidant and calcium wires, the nitrogen content in the smelting process is solved. The nitrogen and carbon content in the smelting process is not qualified. The problem of this paper improves the comprehensive performance and smelting success rate of the alloy, reduces the cost, and meets the chemical composition requirements of ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni-based high-temperature alloys.
Patent Information
- Application Number
- CN202411246098.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-06
AI Technical Summary
When smelting ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni-based high-temperature alloys, the nitrogen content and carbon content are easily unqualified, and the smelting cost is high, making it difficult to meet the chemical composition requirements of the industry standard.
The process route of electric furnace + AOD furnace + LF furnace + electroslag is adopted. By limiting the chemical composition of the raw materials and the conditions of each smelting stage, the nitrogen and carbon content in the alloy is controlled, aluminum and ferrosilicon are used for reduction reactions, oxygen blowing and blowing Nitrogen, deoxidant and calcium wire are added to prevent excessive oxygen content, and finally electroslag remelting is carried out to ensure that the finished product meets the standards.
It effectively avoids the deviation of nitrogen and carbon content, improves the comprehensive performance and smelting success rate of the alloy, reduces the smelting cost, and meets the chemical composition requirements of ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni-based high-temperature alloys.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of alloy smelting, and in particular to a method for smelting an ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloy. Background Art
[0002] Ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloys have good corrosion resistance and high strength, and are suitable for harsh conditions such as chemical engineering and marine environments. They can even be used in highly oxidizing high-concentration inorganic acid media at high temperatures. 015Cr33Ni32MoCuN alloy is an ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloy. The industry standard requires C≤0.015%, N 0.35%~0.60%, and Fe, Cr and Ni elements are all above 30%. The specific composition is shown in Table 1.
[0003] Table 1015 Chemical composition and mass percentage of Cr33Ni32MoCuN alloy (%)
[0004] During the smelting process of high-temperature alloys, segregation is easy to occur due to the high alloying elements. In order to reduce the segregation of alloying elements, high-temperature alloys are generally smelted by the process method of "vacuum induction furnace + electroslag" or "vacuum induction furnace + self-consumable". However, due to the special composition requirements of ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high-temperature alloys, vacuum induction melting has the following disadvantages: the steel has a high nitrogen content. If it is smelted under vacuum, its nitrogen element is very easy to be extracted, resulting in a nitrogen content (mass content) of less than 0.35%; the steel has a low carbon content, and vacuum induction has no decarburization ability. In addition, in order to ensure the nitrogen content, a large amount of chromium nitride needs to be added in the later stage of smelting. Chromium nitride contains a certain amount of carbon, which easily causes carbon to exceed the upper limit of the standard requirements during smelting; in addition, the smelting cost is high. Therefore, it is urgent to find a smelting method suitable for ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high-temperature alloys to meet the corresponding requirements and quality requirements of its chemical composition. Summary of the invention
[0005] In view of the above problems, the present invention provides a smelting method of an ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high-temperature alloy. The present invention adopts the process of "electric furnace + AOD furnace + LF furnace + electroslag". By limiting the chemical composition of raw materials and the conditions of each smelting stage, the nitrogen content and carbon content in the alloy are better controlled, and the ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high-temperature alloy whose chemical composition meets the industry standards is obtained, thereby improving the comprehensive performance of the high-temperature alloy.
[0006] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions: A smelting method of an ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloy comprises the following steps: S1, melting the raw materials in an electric furnace to obtain the first molten steel; The raw materials are prepared according to the following chemical compositions in percentage by mass: Cr 31.75%-34.00%, Ni 30.70%-32.00%, Mo 0.60%-1.00%, Cu 0.60%-0.90%; S2, injecting the first molten steel into an AOD furnace for first refining, blowing oxygen until C≤0.006wt% and Si≤0.01wt%, starting nitrogen blowing throughout the process, adding aluminum and ferrosilicon for reduction reaction, and controlling [Cr]+[Mn]-[Si]≥33% to obtain a second molten steel; Wherein, [Cr] represents the mass content of Cr element, [Mn] represents the mass content of Mn element, and [Si] represents the mass content of Si element; S3, under nitrogen atmosphere, injecting the second molten steel into the LF furnace for second refining, continuously adding deoxidizer for deoxidation during the whole process; adding calcium wire and metal cerium before tapping, to obtain the third molten steel; The deoxidizer is selected from at least one of aluminum wire and aluminum powder; S4, casting the third molten steel to obtain an electrode blank; S5, in a protective atmosphere, electroslag remelting the electrode blank to obtain an ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloy.
[0007] Compared with the prior art, the smelting method of the ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloy provided by the present invention adopts the process route of "electric furnace + AOD furnace + LF furnace + electroslag", which solves the problem of unqualified carbon content and nitrogen content when vacuum induction smelting is adopted, and has high market competitiveness and promotion value. By limiting the content of Cr, Ni, Mo and Cu elements in the ingredients of the raw materials, the present invention can effectively avoid the segregation of each element in the subsequent smelting process or component adjustment, and thus will not increase the smelting time and cause the carbon content to exceed the upper limit; by limiting the comprehensive content of Mn, Cr and Si elements (i.e. [Cr] + [Mn] - [Si]) in the first refining process, the solubility of nitrogen in molten steel is increased, thereby ensuring that the nitrogen content in the alloy meets the standard requirements.
[0008] The present invention creatively carries out nitrogen blowing throughout the first refining process, ensuring that the nitrogen content in the alloy is within the specified range of the industry standard, which not only increases the nitrogen content in the molten steel, but also ensures that the nitrogen content does not exceed 0.60%. The present invention uses nitrogen as a protective gas in the second refining, which can further prevent the reduction of nitrogen; uses aluminum wire or aluminum powder as a deoxidizer and avoids the use of silicon calcium powder, which can further prevent carbon increase; before the steel is tapped in the second refining, the addition of calcium wire and metal cerium can effectively prevent the molten steel from increasing oxygen in the subsequent casting process, thereby ensuring that the oxygen content is qualified. Subsequent electroslag remelting is used to produce an ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high-temperature alloy whose chemical components meet the industry standards, and improves the hot working performance and comprehensive performance of the high-temperature alloy, effectively improving the smelting success rate of the high-temperature alloy.
[0009] Preferably, the ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high-temperature alloy is a 015Cr33Ni32MoCuN alloy, comprising the following chemical components in percentage by mass: C≤0.012%, Si≤0.50%, Mn≤2.00%, P≤0.020%, S≤0.010%, Cr 31.00%~35.00%, Ni 30.00%~33.00%, Mo 0.50%~2.00%, Cu 0.30%~1.20%, N 0.40%~0.47%, and the balance is Fe and unavoidable impurities.
[0010] Preferably, in S1, the raw materials are formulated according to the following chemical compositions in percentage by mass: Mn 0.80%~1.60%, P≤0.018%, Cr 31.75%~34.00%, Ni 30.70%~32.00%, Mo 0.60%~1.00%, Cu 0.60%~0.90%.
[0011] When preparing the ingredients, C and Si elements can be appropriately added in high amounts to prepare for the subsequent oxygen blowing to control the temperature of the molten steel; other chemical components can be conventionally configured according to the above chemical components, and the present invention does not make any requirements.
[0012] Further preferably, in S1, the raw materials are formulated according to the following chemical compositions in percentage by mass: Cr 32.5%, Ni 30.8%, Mo 0.80%, Cu 0.75%.
[0013] The preferred contents of Cr, Ni, Mo and Cu in the ingredients of the present invention can further avoid the segregation of the elements and the resulting unqualified products in the subsequent smelting process or composition adjustment.
[0014] Preferably, in S2, after adding the aluminum and ferrosilicon, the mass content of Si in the molten steel is 0.25%~0.45%, and the mass content of Al is 0.015%~0.045%.
[0015] During the first refining of the first molten steel in the AOD furnace, oxygen is blown to oxidize C and Si elements (the content of Cr element will also be reduced due to oxidation) to ensure the temperature of the first refining; when C≤0.006wt% and Si≤0.01wt% in the molten steel, aluminum and ferrosilicon are added for reduction reaction to return the content of Cr element to the set range, and nitrogen blowing is started throughout the process. At the same time, the content of [Cr]+[Mn]-[Si] is controlled, which can significantly increase the solubility of nitrogen in the molten steel, thereby ensuring that the nitrogen content in the alloy meets the standard requirements.
[0016] Preferably, in S3, the total amount of the deoxidizer added is 0.5 kg / t to 1.5 kg / t.
[0017] For example, in S3, calcium wire and metallic cerium are added 3min to 5min before steel tapping.
[0018] Preferably, in S3, the amount of calcium wire added is 2.8 m / t to 3.2 m / t, and the amount of metal cerium added is 0.2 kg / t to 0.3 kg / t.
[0019] The invention can further effectively prevent the increase of oxygen in the subsequent process by limiting the added amounts of the deoxidizer, the calcium wire and the metal cerium.
[0020] Preferably, in S4, the casting temperature is 1470°C to 1490°C.
[0021] Preferably, in S4, the diameter of the electrode blank is 340 mm to 430 mm.
[0022] Preferably, in S5, the protective atmosphere is a nitrogen atmosphere.
[0023] Preferably, in S5, the slag system used in the electroslag remelting is CaF 2 、Al 2 O 3 , CaO and MgO.
[0024] Further preferably, in S5, the carbon content of the slag system is ≤0.03%.
[0025] Preferably, in S5, the melting rate of the electrode blank is 4.5 kg / min to 7 kg / min.
[0026] Preferably, in S5, the diameter of the ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloy is 480 mm to 590 mm.
[0027] The present invention can further ensure that the chemical composition and gas content of the final electroslag ingot are within a reasonable range through a specific electroslag remelting slag system and a melting rate of the electrode blank, and ensure that the corresponding inclusions can be ≤1.0 level, and ensure that the ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloy has excellent hot working performance and comprehensive performance. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0029] Unless otherwise specified, the percentages in the present invention are all by mass.
[0030] Example 1 This embodiment provides a smelting method of 015Cr33Ni32MoCuN alloy, comprising the following steps: S1, smelting the raw materials in an electric furnace to obtain the first molten steel.
[0031] The raw materials are formulated according to the following chemical composition in percentage by mass: Mn 1.35%, P≤0.018%, Cr32.22%, Ni 31.00%, Mo 0.80%, and Cu 0.70%.
[0032] S2, inject the first molten steel into the AOD furnace for the first refining, blow oxygen until C≤0.006wt% and Si≤0.01wt% in the molten steel, start blowing nitrogen throughout the process, and add aluminum and ferrosilicon for reduction reaction, and adjust elements such as Cr, Ni, Mo and Cu to the internal control range. In this process, Si 0.30%, Mn 1.35%, P≤0.018%, Cr 32.22%, Ni 31.00%, Mo0.80%, Cu 0.70% and Al 0.03% are controlled, [Cr]+[Mn]-[Si]=33.27%, and the second molten steel is obtained.
[0033] S3, under nitrogen atmosphere, the second molten steel is injected into the LF furnace for the second refining, and a total of 1kg / t of aluminum wire is continuously added for deoxidation during the whole process; 3m / t of calcium wire and 0.25kg / t of metallic cerium are added 3min~5min before tapping, and sampling is performed for analysis. After the chemical composition is qualified, the steel is tapped to obtain the third molten steel.
[0034] S4, casting the third molten steel at 1480°C to obtain an electrode blank of Φ380mm.
[0035] S5, in a protective atmosphere, the electrode blank is electroslag remelted, and the slag system used for electroslag remelting is CaF with a mass ratio of 70:20:5:52 、Al 2 O 3 , CaO and MgO, the carbon content of the slag system is ≤0.03%, the melting rate of the electrode blank is 5.6kg / min, and the electroslag ingot of Φ530mm is obtained, which is 015Cr33Ni32MoCuN alloy.
[0036] 015Cr33Ni32MoCuN alloy is composed of the following chemical components in mass percentage: C 0.010%, Si0.30%, Mn 1.35%, P≤0.020%, S≤0.010%, Cr 32.22%, Ni 30.98%, Mo 0.81%, Cu 0.69%, N0.43%, Al 0.02%, O≤20ppm, H≤8ppm, and the balance is Fe and unavoidable impurities.
[0037] Example 2 This embodiment provides a smelting method of 015Cr33Ni32MoCuN alloy, comprising the following steps: S1, smelting the raw materials in an electric furnace to obtain the first molten steel.
[0038] The raw materials are formulated according to the following chemical composition in percentage by mass: Mn 1.60%, P≤0.018%, Cr31.75%, Ni 30.70%, Mo 1.00%, Cu 0.60%, and the balance is Fe and unavoidable impurities.
[0039] S2, inject the first molten steel into the AOD furnace for the first refining, blow oxygen until C≤0.006wt% and Si≤0.01wt% in the molten steel, start blowing nitrogen throughout the process, and add aluminum and ferrosilicon for reduction reaction, adjust the elements such as Cr, Ni, Mo and Cu to the internal control range. In this process, Si 0.25%, Mn 1.60%, P≤0.018%, Cr 31.75%, Ni 30.70%, Mo1.00%, Cu 0.60% and Al 0.045% are controlled, [Cr]+[Mn]-[Si]=33.1%, and the second molten steel is obtained.
[0040] S3, under nitrogen atmosphere, the second molten steel is injected into the LF furnace for the second refining, and a total of 0.5kg / t of aluminum powder is continuously added for deoxidation during the whole process; 2.8m / t of calcium wire and 0.3kg / t of metallic cerium are added 3min~5min before tapping, and sampling is performed for analysis. After the chemical composition is qualified, the steel is tapped to obtain the third molten steel.
[0041] S4, casting the third molten steel at 1470°C to obtain an electrode blank of Φ340 mm.
[0042] S5, in a protective atmosphere, the electrode blank is electroslag remelted. The slag system used for electroslag remelting is CaF with a mass ratio of 68:21:5.5:5.5. 2 、Al 2 O 3 , CaO and MgO, the carbon content of the slag system is ≤0.03%, the melting rate of the electrode blank is 4.5kg / min, and the electroslag ingot of Φ480mm is obtained, which is 015Cr33Ni32MoCuN alloy.
[0043] 015Cr33Ni32MoCuN alloy is composed of the following chemical components in mass percentage: C 0.012%, Si0.25%, Mn 1.74%, P≤0.020%, S≤0.010%, Cr 31.07%, Ni 30.14%, Mo 1.82%, Cu 0.37%, N0.40%, Al 0.045%, O≤23ppm, H≤5ppm, and the balance is Fe and unavoidable impurities.
[0044] Example 3 This embodiment provides a smelting method of 015Cr33Ni32MoCuN alloy, comprising the following steps: S1, smelting the raw materials in an electric furnace to obtain the first molten steel.
[0045] The raw materials are formulated according to the following chemical composition in percentage by mass: Mn 0.80%, P≤0.018%, Cr34.00%, Ni 32.00%, Mo 0.60%, Cu 0.90%, and the balance is Fe and unavoidable impurities.
[0046] S2, inject the first molten steel into the AOD furnace for the first refining, blow oxygen until C≤0.006wt% and Si≤0.01wt% in the molten steel, start blowing nitrogen throughout the process, and add aluminum and ferrosilicon for reduction reaction, adjust the elements such as Cr, Ni, Mo and Cu to the internal control range. In this process, Si 0.45%, Mn 0.80%, P≤0.018%, Cr 34.00%, Ni 32.00%, Mo0.60%, Cu 0.90% and Al 0.015% are controlled, [Cr]+[Mn]-[Si]=34.35%, and the second molten steel is obtained.
[0047] S3, under nitrogen atmosphere, the second molten steel is injected into the LF furnace for the second refining, and 1kg / t of aluminum wire and 0.5kg / t of aluminum powder are continuously added for deoxidation during the whole process; 3min~5min before tapping, 3.2m / t of calcium wire and 0.2kg / t of metallic cerium are added, and sampling is performed for analysis. After the chemical composition is qualified, the steel is tapped to obtain the third molten steel.
[0048] S4, casting the third molten steel at 1490°C to obtain an electrode blank of Φ430mm.
[0049] S5, in a protective atmosphere, the electrode blank is electroslag remelted. The slag system used for electroslag remelting is CaF with a mass ratio of 72:19:4.5:4.5. 2 、Al 2 O 3 , CaO and MgO, the carbon content of the slag system is ≤0.03%, the melting rate of the electrode blank is 7kg / min, and the electroslag ingot of Φ590mm is obtained, which is 015Cr33Ni32MoCuN alloy.
[0050] 015Cr33Ni32MoCuN alloy is composed of the following chemical components in mass percentage: C 0.010%, Si0.45%, Mn 0.80%, P≤0.020%, S≤0.010%, Cr 34.82%, Ni 32.57%, Mo 0.53%, Cu 1.15%, N0.46%, Al 0.02%, O≤20ppm, H≤6ppm, and the balance is Fe and unavoidable impurities.
[0051] Example 4 This embodiment provides a smelting method of 015Cr33Ni32MoCuN alloy, comprising the following steps: S1, smelting the raw materials in an electric furnace to obtain the first molten steel.
[0052] The raw materials are formulated according to the following chemical composition in percentage by mass: Mn 1.13%, P≤0.018%, Cr32.45%, Ni 31.15%, Mo 0.88%, Cu 0.69%, and the balance is Fe and unavoidable impurities.
[0053] S2, inject the first molten steel into the AOD furnace for the first refining, blow oxygen until C≤0.006wt% and Si≤0.01wt% in the molten steel, start blowing nitrogen throughout the process, and add aluminum and ferrosilicon for reduction reaction, and adjust elements such as Cr, Ni, Mo and Cu to the internal control range. In this process, Si 0.40%, Mn 1.13%, P≤0.018%, Cr 32.45%, Ni 31.15%, Mo0.88%, Cu 0.69% and Al 0.02% are controlled, [Cr]+[Mn]-[Si]=33.27%, and the second molten steel is obtained.
[0054] S3, under nitrogen atmosphere, the second molten steel is injected into the LF furnace for the second refining, and a total of 1kg / t of aluminum wire is continuously added for deoxidation during the whole process; 3m / t of calcium wire and 0.25kg / t of metallic cerium are added 3min~5min before tapping, and sampling is performed for analysis. After the chemical composition is qualified, the steel is tapped to obtain the third molten steel.
[0055] S4, casting the third molten steel at 1480°C to obtain an electrode blank of Φ390 mm.
[0056] The electrode blank is composed of the following chemical components in percentage by mass: C 0.012%, Si 0.40%, Mn 1.13%, P≤0.020%, S≤0.010%, Cr 32.45%, Ni 31.12%, Mo 0.85%, Cu 0.67%, N 0.41%, Al 0.02%, O≤22ppm, H≤7ppm, and the balance is Fe and unavoidable impurities.
[0057] S5: Electroslag remelting of the electrode blank is carried out under protective atmosphere. The slag system used for electroslag remelting is CaF with a mass ratio of 70:15:15. 2 、Al 2 O 3 and CaO, the melting rate of the electrode blank is 5.8kg / min, and the electroslag ingot of Φ540mm is obtained, which is 015Cr33Ni32MoCuN alloy.
[0058] 015Cr33Ni32MoCuN alloy is composed of the following chemical components in mass percentage: C 0.016%, Si0.40%, Mn 1.13%, P≤0.020%, S≤0.010%, Cr 32.45%, Ni 31.12%, Mo 0.85%, Cu 0.67%, N0.41%, Al 0.02%, O≤22ppm, H≤7ppm, and the balance is Fe and unavoidable impurities.
[0059] Comparative Example 1 This comparative example provides a smelting method of 015Cr33Ni32MoCuN alloy, which adopts a vacuum induction smelting method and includes the following steps: The vacuum induction furnace (1t) uses pure metal ingredients. The mid-term inspection of smelting shows C 0.005% and N 0.004%. After the other chemical components are appropriate, argon is filled with 10000Pa in the later stage of smelting, and nitrogen is increased by adding chromium nitride. The chromium nitride contains about 3% N. 150kg of chromium nitride is added to finally obtain a Φ380mm electrode blank.
[0060] The obtained electrode blank was tested for chemical composition and was composed of the following chemical components in mass percentage: C 0.018%, Si 0.40%, Mn 1.70%, P≤0.020%, S≤0.010%, Cr 33.07%, Ni 30.65%, Mo 0.88%, Cu 0.73%, N 0.24%, Al 0.02%, O 15ppm, H 0.5ppm, and the balance was Fe and unavoidable impurities.
[0061] Because the C element exceeded the upper limit and the N element was below the lower limit, the chemical composition was unqualified and production was stopped.
[0062] Comparative Example 2 This comparative example provides a smelting method of 015Cr33Ni32MoCuN alloy, which is similar to Example 1, except that: in S2, Cr is 31.45%, Mn is 1.04%, Si is 0.43%, [Cr]+[Mn]-[Si]=32.06. The remaining conditions are the same as those in Example 1 and will not be described in detail.
[0063] The chemical composition of the third molten steel was tested and it was found that the N content was only 0.34%. The chemical composition was unqualified and production was stopped.
[0064] Comparative Example 3 This comparative example provides a smelting method of 015Cr33Ni32MoCuN alloy, which is similar to Example 1, except that in S3, the aluminum wire is replaced with calcium silicon powder of the same mass. The remaining conditions are the same as those in Example 1 and will not be described in detail.
[0065] The chemical composition of the third molten steel was tested, and it was found that the content of C element gradually increased to 0.017% before steelmaking. The chemical composition was unqualified, and production was stopped.
[0066] Comparative Example 4 This comparative example provides a smelting method of 015Cr33Ni32MoCuN alloy, which is similar to Example 1, except that in S3, only calcium wire is added and metal cerium is omitted. The remaining conditions are the same as those in Example 1 and will not be described in detail.
[0067] 015Cr33Ni32MoCuN alloy is composed of the following chemical components in mass percentage: C 0.010%, Si0.30%, Mn 1.35%, P≤0.020%, S≤0.010%, Cr 32.22%, Ni 30.98%, Mo 0.81%, Cu 0.69%, N0.43%, Al 0.02%, O≤32ppm, H≤8ppm, and the balance is Fe and unavoidable impurities.
[0068] During the later forging process, many cracks appeared on the surface of the 015Cr33Ni32MoCuN alloy, which resulted in a low yield and increased cost.
[0069] Comparative Example 5 This comparative example provides a smelting method of 015Cr33Ni32MoCuN alloy, which is similar to Example 1, except that in S2, nitrogen is blown only in the first half. The remaining conditions are the same as those in Example 1 and will not be described in detail.
[0070] The chemical composition of the third molten steel was tested. The nitrogen content of the AOD furnace sample was 0.4%, and the nitrogen content of the LF furnace sample gradually decreased to 0.32%. The chemical composition was unqualified and production was stopped.
[0071] Performance Testing The present invention performs inclusion level test and mechanical property test on the 015Cr33Ni32MoCuN alloy prepared in Examples 1 to 4 and Comparative Example 4, respectively (test standard reference GB / T 228.1-2021), and the test results are shown in Tables 2 to 3. As can be seen from Tables 2 to 3, compared with Examples 1 to 3, the electroslag remelting slag system of Example 4 contains more CaO, and CaO contains a small amount of carbon, so the C at the bottom of the electroslag ingot is 0.016%, which cannot meet the standard requirements, resulting in low yield and increased cost.
[0072] Table 2 Inclusion levels of 015Cr33Ni32MoCuN alloys of Examples 1 to 4 and Comparative Example 4
[0073] Table 3 Mechanical properties test results of 015Cr33Ni32MoCuN alloy of Examples 1 to 4 and Comparative Example 4
[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for smelting ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloy, characterized in that: The following steps are involved: S1, melting the raw materials in an electric furnace to obtain the first molten steel; The raw materials are prepared according to the following chemical compositions in percentage by mass: Cr 31.75%-34.00%, Ni 30.70%-32.00%, Mo 0.60%-1.00%, Cu 0.60%-0.90%; S2, injecting the first molten steel into an AOD furnace for first refining, blowing oxygen until C≤0.006wt% and Si≤0.01wt%, starting nitrogen blowing throughout the process, adding aluminum and ferrosilicon for reduction reaction, and controlling [Cr]+[Mn]-[Si]≥33% to obtain a second molten steel; Wherein, [Cr] represents the mass content of Cr element, [Mn] represents the mass content of Mn element, and [Si] represents the mass content of Si element; S3, under nitrogen atmosphere, injecting the second molten steel into the LF furnace for second refining, continuously adding deoxidizer for deoxidation during the whole process; adding calcium wire and metal cerium before tapping, to obtain the third molten steel; The deoxidizer is selected from at least one of aluminum wire and aluminum powder; S4, casting the third molten steel to obtain an electrode blank; S5, in a protective atmosphere, electroslag remelting the electrode blank to obtain an ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloy.
2. The smelting method of the ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloy according to claim 1, characterized in that: The ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloy is a 015Cr33Ni32MoCuN alloy, comprising the following chemical components in percentage by mass: C≤0.012%, Si≤0.50%, Mn≤2.00%, P≤0.020%, S≤0.010%, Cr 31.00%~35.00%, Ni 30.00%~33.00%, Mo 0.50%~2.00%, Cu 0.30%~1.20%, N 0.40%~0.47%, and the balance is Fe and unavoidable impurities.
3. The smelting method of the ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloy according to claim 1, characterized in that: In S1, the raw materials are formulated according to the following chemical compositions in percentage by mass: Mn 0.80%~1.60%, P≤0.018%, Cr31.75%~34.00%, Ni 30.70%~32.00%, Mo 0.60%~1.00%, and Cu 0.60%~0.90%.
4. The smelting method of the ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloy according to claim 1, characterized in that: In S2, after adding the aluminum and ferrosilicon, the mass content of Si in the molten steel is 0.25%~0.45%, and the mass content of Al is 0.015%~0.045%.
5. The smelting method of the ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloy according to claim 1, characterized in that: In S3, the total amount of the deoxidizer added is 0.5kg / t to 1.5kg / t.
6. The smelting method of the ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloy according to claim 1, characterized in that: In S3, the amount of calcium wire added is 2.8m / t~3.2m / t, and the amount of metal cerium added is 0.2kg / t~0.3kg / t.
7. The smelting method of the ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloy according to claim 1, characterized in that: In S4, the casting temperature is 1470°C to 1490°C.
8. The smelting method of the ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloy according to claim 1, characterized in that: In S5, the slag system used in the electroslag remelting is CaF2, Al2O3, CaO and MgO in a mass ratio of (68~72):(19~21):(4.5~5.5):(4.5~5.5); the carbon content of the slag system is ≤0.03%.
9. The smelting method of the ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloy according to claim 1, characterized in that: In S4, the diameter of the electrode blank is 340 mm to 430 mm.
10. The smelting method of the ultra-high nitrogen and ultra-low carbon Fe-Cr-Ni based high temperature alloy according to claim 1 or 9, characterized in that: In S5, the protective atmosphere is a nitrogen atmosphere; and the melting rate of the electrode blank is 4.5 kg / min to 7 kg / min.
Citation Information
Patent Citations
Phosphorus-controlled 00Cr21Ni13Mn5N high-nitrogen austenitic stainless steel and production method thereof
CN117660849A
Special wire rod for manufacturing stainless steel wire in marine environment and preparation method of special wire rod
CN117867397A
Method of making Cr alloy workpieces and its use
CN1221802A