Heat treatment method for prolonging service life of high-speed steel roller

Through the heat treatment method of gradual heating and cooling, the problem of cracking of high-speed steel rolls during the heat treatment process is solved, the service life and performance of the rolls are improved, the cracking problems during the heat treatment process is avoided, and the efficient performance of the rolls is improved.

CN119040607APending Publication Date: 2024-11-29BAOGANG GRP METALLURGY ROLLER MFG CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411279556.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

High-speed steel rolls are prone to cracking during heat treatment, resulting in shortening of service life, and the heat treatment process is complex and difficult to monitor, which can easily lead to batch cracking and economic losses.

Method used

A heat treatment method is adopted, including step-by-step heating and cooling process, the specific steps are: initial heat to 100~140℃, insulation, gradually heating to 530~570℃, 630~700℃, 760~800℃, 860~900℃ and 990 ~1030℃, and insulated in the high-temperature section, then cooled and undergo three tempering treatments, adjusting the quenching temperature and cooling method to affect the crystal structure and performance.

Benefits of technology

By adjusting the heat treatment temperature and cooling method, the service life of high-speed steel rolls is significantly improved, cracking problems during the heat treatment process is avoided, and the working layer and core performance of the rolls is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040607A_ABST
    Figure CN119040607A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of roller casting, and discloses a heat treatment method for prolonging the service life of a high-speed steel roller, which comprises the following steps of: 1, heating a furnace to 120 DEG C when the initial temperature in a high-speed steel roller chamber is 20 DEG C, and putting the high-speed steel roller into the furnace; the high-speed steel roller is subjected to heat preservation for 4 hours at the temperature of 120 DEG C; then heating the high-speed steel roller from 120 DEG C to 550 DEG C for 20 hours, and keeping the temperature for 8 hours at the temperature of 550 DEG C; heating the high-speed steel roller from 550 DEG C to 650 DEG C for 6 hours, and preserving heat for 12 hours at the temperature of 650 DEG C to finish the preheating process of the high-speed steel roller; the heat treatment disclosed by the invention can improve the performance of the high-speed steel roller, the crystal structure and performance of the roller are influenced by adjusting the quenching temperature, the cooling mode, the tempering temperature and the tempering frequency in the heat treatment process, the performance of a working layer and the performance of a core part of the high-speed steel roller are remarkably influenced, and the cracking problem in the heat treatment process is avoided; and the service life of the high-speed steel roller is greatly prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of roll casting, and in particular to a heat treatment method for improving the service life of a high-speed steel roll. Background Art

[0002] Rollers are essential and vulnerable parts in steel rolling production. The quality of rolls directly affects the quality of steel. Centrifugally composite cast high-speed steel rolls have good wear resistance and thermal crack resistance and are one of the important products of modern rolls.

[0003] During the production and use of high-speed steel rolls, cracking is the most common quality accident, accounting for about 60% of the total accidents. Cracking can be divided into hot cracking, cold cracking and cracking during heat treatment.

[0004] The causes of thermal cracking include: during centrifugal casting, the cold mold temperature is too low or the casting temperature is too low; the pouring process is unstable or vibrates violently; the core metal liquid is deflected or scattered during top pouring; the riser part solidifies prematurely, and the solidified roller shell layer cannot withstand the tension of graphitization expansion during the solidification of the core.

[0005] The causes of cold cracking include: when the roll is cooled below the elastic state of the metal, the internal stress is too large or the contraction is hindered; the roll is opened too early, and the thermal stress and the phase change stress of the rapid transformation of austenite to martensite are superimposed; uneven cooling of the roll in the mold or after opening the mold, as well as local overheating can cause cold cracking.

[0006] The causes of cracking during heat treatment include: too fast heating or uneven heating or cooling speed; excessive residual stress of the roll accompanied by phase change stress during heat treatment; poor organization caused by improper preliminary heat treatment.

[0007] Hot cracking and cold cracking can be controlled through observation and detection in the production process. Hot cracking and cold cracking usually occur in a single roll and are relatively easy to prevent. However, the heat treatment process is carried out in a closed kiln, and it is not easy to monitor the entire process. In addition, the heat treatment cycle of high-speed steel rolls is longer and the process is more complicated than that of other rolls. During the heat treatment process, it is very easy to crack due to changes in the internal metallographic structure and internal stress release. Heat treatment cracking is usually treated in one kiln for multiple rolls, which is prone to batch cracking and high economic losses. Summary of the invention

[0008] The purpose of the present invention is to provide a heat treatment method for increasing the service life of a high-speed steel roll, and to solve the problem of cracking of the high-speed steel roll during the heat treatment process mentioned in the above background technology.

[0009] The technical solution adopted by the present invention is as follows: A heat treatment method for improving the service life of a high-speed steel roll comprises the following steps: Step 1: The initial temperature in the high-speed steel roller room is 20℃. Heat the furnace to 100~140℃ and put the high-speed steel roller into the furnace. First, keep the high-speed steel roller at 100~140℃ for 3~5 hours. Then heat the high-speed steel roller from 100~140℃ to 530~570℃ for 19~21 hours and keep it at 530~570℃ for 7~9 hours. Then heat the high-speed steel roller from 530~570℃ to 630~700℃ for 5~7 hours and keep it at 630~700℃ for 11~13 hours to complete the preheating process of the high-speed steel roller. Step 2: Heat the high-speed steel roll from 630-700°C to 760-800°C for 3-5 hours, then heat from 760-800°C to 860-900°C for 19-21 hours, then heat from 860-900°C to 990-1030°C for 11-13 hours, and keep at 990-1030°C for 5-7 hours to complete the high-temperature section of the high-speed steel roll; Step 3: After the high-speed steel roller is kept at 990~1030℃ for 5~7 hours, the high-temperature heating process is completed and the cooling process begins; the first stage of cooling adopts air cooling; when the surface temperature of the roller working layer drops to 630~670℃, the air cooling is changed to air blowing cooling; when the surface temperature of the high-speed steel roller working layer drops to 470~500℃, the air blowing cooling is stopped; the second air cooling is carried out; when the surface temperature of the high-speed steel roller working layer drops to 450~470℃, the air cooling is stopped; the cooling process of the high-speed steel roller is completed; Step 4: When the high-speed steel roll is air-cooled to 410~450℃ and the cooling process is completed, the high-speed steel roll is tempered; first, the high-speed steel roll is heated from 410~450℃ to 470~490℃ for 3~5 hours, and kept at 470~490℃ for 5~7 hours; then the temperature is lowered to 240~260℃, and then heated to 500~540℃ for 29~31 hours, and kept at 500~540℃ for 9~11 hours; then the temperature is lowered to After 90~110℃, keep warm for 5~7 hours; heat to 500~540℃ for 41~43 hours, and keep warm at 500~540℃ for 17~19 hours; then start to cool down, keep warm for 5~7 hours after cooling to 90~110℃, heat to 500~540℃ for 41~43 hours, and keep warm at 500~540℃ for 17~19 hours; then start to cool down, the surface of the working layer of the high-speed steel roll drops to 110~130℃ and takes out of the furnace, and the three tempering of the high-speed steel roll is completed.

[0010] The beneficial effects of the present invention are as follows: the heat treatment disclosed in the present application can improve the performance of the high-speed steel roll, and the heat treatment process affects the crystal structure and performance of the roll by adjusting the quenching temperature, cooling method, tempering temperature and tempering times, and has a significant impact on the working layer performance and core performance of the high-speed steel roll, thereby avoiding the cracking problem during the heat treatment process and greatly improving the service life of the high-speed steel roll. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 This is a schematic diagram of the process flow of step 1 in Example 2.

[0012] Figure 2 This is a schematic diagram of the process flow of step 2 in Example 2.

[0013] Figure 3 This is a schematic diagram of the process flow of step 4 in Example 2.

[0014] Figure 4 To improve the metallographic structure of the front roll body.

[0015] Figure 5 To improve the metallographic structure of the roller body. DETAILED DESCRIPTION

[0016] To facilitate those skilled in the art to understand the present invention, specific implementations of the present invention are described below with reference to the accompanying drawings.

[0017] like Figure 4 As shown, the metallographic structure of the roller body before improvement is disclosed.

[0018] like Figure 5 As shown, the improved metallographic structure of the roller body is disclosed.

[0019] A heat treatment method for increasing the service life of a high-speed steel roll comprises the following steps: Step 1: The initial temperature in the high-speed steel roller room is 20℃. Heat the furnace to 100~140℃ and put the high-speed steel roller into the furnace. First, keep the high-speed steel roller at 100~140℃ for 3~5 hours. Then heat the high-speed steel roller from 100~140℃ to 530~570℃ for 19~21 hours and keep it at 530~570℃ for 7~9 hours. Then heat the high-speed steel roller from 530~570℃ to 630~700℃ for 5~7 hours and keep it at 630~700℃ for 11~13 hours to complete the preheating process of the high-speed steel roller. Since the heating speed of the high-speed steel roll is slightly slower at low temperatures and slightly faster at high temperatures, the preheating process can reduce the casting stress of the high-speed steel roll, and can increase the working layer and core temperature of the high-speed steel roll to about 650°C, thereby improving the heating efficiency of the high-speed steel roll and reducing the overall heat content of the high-speed steel roll, thus preparing for the differential temperature heating process; making the high-speed steel roll reach above the elastic-plastic transition temperature and enter the plastic zone to adapt to the subsequent rapid heating process; Step 2: Heat the high-speed steel roll from 630-700°C to 760-800°C for 3-5 hours, then heat from 760-800°C to 860-900°C for 19-21 hours, then heat from 860-900°C to 990-1030°C for 11-13 hours, and keep at 990-1030°C for 5-7 hours to complete the high-temperature section of the high-speed steel roll; Since the high-temperature heating and cooling process of the high-speed steel roll is the core process to improve the performance of the high-speed steel roll, it is the most critical step in the entire heat treatment process; therefore, the austenitizing temperature of the high-speed steel in this application is 970-1020°C, and the minimum is not less than 945°C. If the temperature is lower than 945°C, the dissolved carbon and alloy in the austenite are insufficient, and the quenching hardness of the high-speed steel will be affected; the maximum temperature is not higher than 1045°C. If the temperature is higher than 1045°C, the austenite in the working layer will increase significantly, which will have an adverse effect on the toughness and hardness of the working layer; Step 3: After the high-speed steel roller is kept at 990~1030℃ for 5~7 hours, the high-temperature heating process is completed and the cooling process begins; the first stage of cooling adopts air cooling. In the initial stage of air cooling, the cooling speed of the high-speed steel roller is relatively fast. As the air cooling proceeds, the cooling speed of the high-speed steel roller gradually decreases; when the surface temperature of the roller working layer drops to 630~670℃, the air cooling is changed to air blowing cooling to speed up the cooling speed of the high-speed steel roller again, in order to prevent the pearlite transformation of the working layer of the high-speed steel roller; when the surface temperature of the working layer of the high-speed steel roller drops to 470~500℃, the air blowing cooling is stopped; the second air cooling is carried out to make the temperature inside and outside the working layer of the high-speed steel roller uniform; when the surface temperature of the working layer of the high-speed steel roller drops to 450~470℃, the air cooling is stopped; the cooling process of the high-speed steel roller is completed; Step 4: When the high-speed steel roller is air-cooled to 410~450℃ and the cooling process is completed, the high-speed steel roller is tempered; first, the high-speed steel roller is heated from 410~450℃ to 470~490℃ for 3~5 hours, and kept at 470~490℃ for 5~7 hours; then the temperature is lowered to 240~260℃ (this can prevent the increase of martensite in the high-speed steel roller and avoid affecting the performance of the high-speed steel roller, so it is not cooled to room temperature), and then heated to 500~540℃ for 29~31 hours, and kept at 500~540℃ for 9~11 hours; then the temperature is lowered to 9 After 0~110℃, keep warm for 5~7 hours (keeping warm during tempering causes martensite to begin to decompose, and the supersaturation of residual austenite in the keeping warm process gradually decreases); then heat to 500~540℃ for 41~43 hours, and keep warm at 500~540℃ for 17~19 hours; then start cooling, keep warm for 5~7 hours after cooling to 90~110℃, then heat to 500~540℃ for 41~43 hours, and keep warm at 500~540℃ for 17~19 hours; then start cooling, the surface of the working layer of the high-speed steel roll drops to 110~130℃ and then it is taken out of the furnace, and the three tempering of the high-speed steel roll is completed; Among them, the chemical composition of the working layer of the high-speed steel roll is C 1.2-1.5; Si is 0.8-1.5; Mn is <0.5; P is <0.03; S is <0.02; Ni is 0.5-0.8; Cr is 4.0-5.5; Mo is 4.0-5.0; W is 2.0-2.1; V is 3.0-4.2; Nb is 0.6-0.7; Among them, the core chemical composition of the high-speed steel roll is C 2.8-3.0; Si is 2.4-2.5; Mn is 0.6-0.7; P is <0.1; S is <0.03; Cr is <0.3; Mg is ≥0.04.

[0020] Table 1 and Table 2 are the main mechanical properties statistics of the products

[0021] Table 1 shows the performance indicators of the improved products

[0022] Table 2 shows the product performance indicators before improvement The present invention will be further described below through specific embodiments.

[0023] Embodiment 1, step 1: the initial temperature in the high-speed steel roll chamber is 20°C, the furnace is heated to 100°C, and the high-speed steel roll is placed in the furnace; the high-speed steel roll is first kept at 100°C for 3 hours; then the high-speed steel roll is heated from 100°C to 530°C for 19 hours, and kept at 530°C for 7 hours; then the high-speed steel roll is heated from 530°C to 630°C for 5 hours, and kept at 630°C for 11 hours, completing the preheating process of the high-speed steel roll; Step 2: Heat the high-speed steel roll from 630°C to 760°C for 3 hours, then heat from 760°C to 860°C for 19 hours, then heat from 860°C to 990°C for 11 hours, and keep warm at 990°C for 5 hours to complete the high-temperature section of the high-speed steel roll; Step 3: After the high-speed steel roll is kept at 990℃ for 5 hours, the high-temperature heating process is completed and the cooling process begins; the first stage of cooling adopts air cooling; when the surface temperature of the working layer of the roll drops to 630℃, the air cooling is changed to air blowing cooling; when the surface temperature of the working layer of the high-speed steel roll drops to 470℃, the air blowing cooling is stopped; the second air cooling is carried out; when the surface temperature of the working layer of the high-speed steel roll drops to 450℃, the air cooling is stopped; the cooling process of the high-speed steel roll is completed; Step 4: When the high-speed steel roller is air-cooled to 410°C and the cooling process is completed, the high-speed steel roller is tempered; first, the high-speed steel roller is heated from 410°C to 470°C for 3 hours, and kept at 470°C for 5 hours; then the temperature is lowered, and after it drops to 240°C, it is heated to 500°C for 29 hours, and kept at 500°C for 9 hours; then the temperature is lowered, and it is kept at 90°C for 5 hours; then it is heated to 500°C for 41 hours, and kept at 500°C for 17 hours; then the temperature is lowered, and it is kept at 90°C for 5 hours, and then it is heated to 500°C for 41 hours, and kept at 500°C for 17 hours; then the temperature is lowered, and the surface of the working layer of the high-speed steel roller drops to 110°C and is taken out of the furnace, and the three temperings of the high-speed steel roller are completed.

[0024] Embodiment 2, step 1: the initial temperature in the high-speed steel roll chamber is 20°C, the furnace is heated to 120°C, and the high-speed steel roll is placed in the furnace; the high-speed steel roll is first kept at 120°C for 4 hours; then the high-speed steel roll is heated from 120°C to 550°C for 20 hours, and kept at 550°C for 8 hours; then the high-speed steel roll is heated from 550°C to 650°C for 6 hours, and kept at 650°C for 12 hours, completing the preheating process of the high-speed steel roll; the process flow diagram of the process is shown in Figure 1 As shown; Step 2: Heat the high-speed steel roll from 650°C to 780°C for 4 hours, then heat from 780°C to 880°C for 20 hours, then heat from 880°C to 1010°C for 12 hours, keep warm at 1010°C for 6 hours to complete the high-temperature section of the high-speed steel roll; the process flow diagram of this process is as follows Figure 2 As shown; Step 3: After the high-speed steel roll is kept at 1010℃ for 6 hours, the high-temperature heating process is completed and the cooling process begins; the first stage of cooling adopts air cooling; when the surface temperature of the working layer of the roll drops to 650℃, the air cooling is changed to air blowing cooling; when the surface temperature of the working layer of the high-speed steel roll drops to 480℃, the air blowing cooling is stopped; the second air cooling is carried out; when the surface temperature of the working layer of the high-speed steel roll drops to 465℃, the air cooling is stopped; the cooling process of the high-speed steel roll is completed; Step 4: When the high-speed steel roller is air-cooled to 420°C and the cooling process is completed, the high-speed steel roller is tempered; first, the high-speed steel roller is heated from 420°C to 480°C for 4 hours, and kept at 480°C for 6 hours; then the temperature is lowered, and after it drops to 250°C, it is heated to 520°C for 30 hours, and kept at 520°C for 10 hours; then the temperature is lowered, and it is kept at 100°C for 6 hours; then it is heated to 520°C for 42 hours, and kept at 520°C for 18 hours; then the temperature is lowered, and it is kept at 100°C for 6 hours, and then it is heated to 520°C for 42 hours, and kept at 520°C for 18 hours; then the temperature is lowered, and the surface of the working layer of the high-speed steel roller drops to 120°C and is taken out of the furnace. The three temperings of the high-speed steel roller are completed. The process flow diagram of this process is as follows Figure 3 shown.

[0025] Embodiment 3, step 1: the initial temperature in the high-speed steel roll chamber is 20°C, the furnace is heated to 140°C, and the high-speed steel roll is placed in the furnace; the high-speed steel roll is first kept at 140°C for 5 hours; then the high-speed steel roll is heated from 140°C to 570°C for 21 hours, and kept at 570°C for 9 hours; then the high-speed steel roll is heated from 570°C to 700°C for 7 hours, and kept at 700°C for 13 hours, completing the preheating process of the high-speed steel roll; Step 2: Heat the high-speed steel roll from 700°C to 800°C for 5 hours, then heat from 800°C to 900°C for 21 hours, then heat from 900°C to 1030°C for 13 hours, keep warm at 1030°C for 7 hours, and complete the high-temperature section of the high-speed steel roll; Step 3: After the high-speed steel roller is kept at 1030℃ for 7 hours, the high-temperature heating process is completed and the cooling process begins; the first stage of cooling adopts air cooling; when the surface temperature of the roller working layer drops to 670℃, the air cooling is changed to air blowing cooling; when the surface temperature of the high-speed steel roller working layer drops to 500℃, the air blowing cooling is stopped; the second air cooling is carried out; when the surface temperature of the high-speed steel roller working layer drops to 470℃, the air cooling is stopped; the cooling process of the high-speed steel roller is completed; Step 4: When the high-speed steel roller is air-cooled to 450°C and the cooling process is completed, the high-speed steel roller is tempered; first, the high-speed steel roller is heated from 450°C to 490°C for 5 hours, and kept at 490°C for 7 hours; then the temperature is lowered, and after it drops to 260°C, it is heated to 540°C for 31 hours, and kept at 540°C for 11 hours; then the temperature is lowered, and it is kept at 110°C for 7 hours; then it is heated to 540°C for 43 hours, and kept at 540°C for 19 hours; then the temperature is lowered, and it is kept at 110°C for 7 hours, and then it is heated to 540°C for 43 hours, and kept at 540°C for 19 hours; then the temperature is lowered, and the surface of the working layer of the high-speed steel roller drops to 130°C and is taken out of the furnace, and the three temperings of the high-speed steel roller are completed.

[0026] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. The protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A heat treatment method for increasing the service life of a high-speed steel roll, comprising the following steps: Step 1: Heat the furnace to 100~140℃, and put the high-speed steel roll into the furnace; first, keep the high-speed steel roll at 100~140℃ for 3~5 hours; then heat the high-speed steel roll from 100~140℃ to 530~570℃ for 19~21 hours, and keep it at 530~570℃ for 7~9 hours; then heat the high-speed steel roll from 530~570℃ to 630~700℃ for 5~7 hours, and keep it at 630~700℃ for 11~13 hours, thus completing the preheating process of the high-speed steel roll; Step 2: Heat the high-speed steel roll from 630-700°C to 760-800°C for 3-5 hours, then heat from 760-800°C to 860-900°C for 19-21 hours, then heat from 860-900°C to 990-1030°C for 11-13 hours, and keep at 990-1030°C for 5-7 hours to complete the high-temperature section of the high-speed steel roll; Step 3: After the high-speed steel roll is kept at 990~1030℃ for 5~7 hours, the high-temperature heating process is completed and the cooling process begins; the first stage of cooling adopts air cooling; when the surface temperature of the working layer of the roll drops to 630~670℃, the air cooling is changed to air cooling; when the surface temperature of the working layer of the high-speed steel roll drops to 470~500℃, the air cooling is stopped; Carry out the second air cooling; when the surface temperature of the working layer of the high-speed steel roll drops to 450~470℃, stop air cooling; the cooling process of the high-speed steel roll is completed; Step 4: When the high-speed steel roll is air-cooled to 410-450°C, after the cooling process is completed, the high-speed steel roll is tempered; first, the high-speed steel roll is heated from 410-450°C to 470-490°C for 3-5 hours, and kept at 470-490°C for 5-7 hours; then the temperature is lowered to 240 ~260℃, then heat to 500~540℃, it takes 29~31 hours, and keep it at 500~540℃ for 9~11 hours; then start to cool down, keep it at 90~110℃ for 5~7 hours; then heat to 500~540℃, it takes 41~43 hours, and keep it at 500~540℃ for 17~19 hours; then start to cool down, keep it at 90~110℃ for 5~7 hours, then heat to 500~540℃, it takes 41~43 hours, and keep it at 500~540℃ for 17~19 hours; then start to cool down, the surface of the working layer of the high-speed steel roll drops to 110~130℃ and then it is taken out of the furnace, and the three tempering of the high-speed steel roll is completed.

2. A heat treatment method for increasing the service life of a high-speed steel roll according to claim 1, characterized in that: The chemical composition of the working layer of the high-speed steel roll is C 1.2-1.5; Si is 0.8-1.5; Mn is <0.5; P is <0.03; S is <0.02; Ni is 0.5-0.8; Cr is 4.0-5.5; Mo is 4.0-5.0; W is 2.0-2.1; V is 3.0-4.2; Nb is 0.6-0.

7.

3. A heat treatment method for increasing the service life of a high-speed steel roll according to claim 2, characterized in that: The core chemical composition of the high-speed steel roll is C 2.8-3.0; Si is 2.4-2.5; Mn is 0.6-0.7; P is <0.1; S is <0.03; Cr is <0.3; Mg is ≥0.

04.

4. A heat treatment method for increasing the service life of a high-speed steel roll according to claim 1, characterized in that: The initial temperature of the high-speed steel roll chamber is 20°C.

5. A heat treatment method for increasing the service life of a high-speed steel roll according to claim 1, characterized in that: Step 1: The initial temperature in the high-speed steel roll chamber is 20°C. The furnace is heated to 100°C and the high-speed steel roll is placed in the furnace. The high-speed steel roll is first kept at 100°C for 3 hours. Then the high-speed steel roll is heated from 100°C to 530°C for 19 hours and kept at 530°C for 7 hours. Then the high-speed steel roll is heated from 530°C to 630°C for 5 hours and kept at 630°C for 11 hours to complete the preheating process of the high-speed steel roll. Step 2: Heat the high-speed steel roll from 630°C to 760°C for 3 hours, then heat from 760°C to 860°C for 19 hours, then heat from 860°C to 990°C for 11 hours, and keep warm at 990°C for 5 hours to complete the high-temperature section of the high-speed steel roll; Step 3: After the high-speed steel roll is kept at 990℃ for 5 hours, the high-temperature heating process is completed and the cooling process begins; the first stage of cooling adopts air cooling; when the surface temperature of the working layer of the roll drops to 630℃, the air cooling is changed to air cooling; when the surface temperature of the working layer of the high-speed steel roll drops to 470℃, the air cooling is stopped; Carry out the second air cooling; when the surface temperature of the working layer of the high-speed steel roll drops to 450°C, stop air cooling; the cooling process of the high-speed steel roll is completed; Step 4: When the high-speed steel roller is air-cooled to 410°C and the cooling process is completed, the high-speed steel roller is tempered; first, the high-speed steel roller is heated from 410°C to 470°C for 3 hours, and kept at 470°C for 5 hours; then the temperature is lowered, and after it drops to 240°C, it is heated to 500°C for 29 hours, and kept at 500°C for 9 hours; then the temperature is lowered, and it is kept at 90°C for 5 hours; then it is heated to 500°C for 41 hours, and kept at 500°C for 17 hours; then the temperature is lowered, and it is kept at 90°C for 5 hours, and then it is heated to 500°C for 41 hours, and kept at 500°C for 17 hours; then the temperature is lowered, and the surface of the working layer of the high-speed steel roller drops to 110°C and is taken out of the furnace, and the three temperings of the high-speed steel roller are completed.

6. A heat treatment method for increasing the service life of a high-speed steel roll according to claim 1, characterized in that: Step 1: The initial temperature in the high-speed steel roller chamber is 20℃. Heat the furnace to 120℃ and put the high-speed steel roller into the furnace. First, keep the high-speed steel roller at 120℃ for 4 hours. Then heat the high-speed steel roller from 120℃ to 550℃ for 20 hours and keep it at 550℃ for 8 hours. Then heat the high-speed steel roller from 550℃ to 650℃ for 6 hours and keep it at 650℃ for 12 hours to complete the preheating process of the high-speed steel roller.

7. A heat treatment method for increasing the service life of a high-speed steel roll according to claim 1, characterized in that: Step 2: Heat the high-speed steel roller from 650°C to 780°C for 4 hours, then heat it from 780°C to 880°C for 20 hours, then heat it from 880°C to 1010°C for 12 hours, keep it at 1010°C for 6 hours to complete the high-temperature section process of the high-speed steel roller.

8. A heat treatment method for increasing the service life of a high-speed steel roll according to claim 1, characterized in that: Step 3: After the high-speed steel roll is kept at 1010℃ for 6 hours, the high-temperature heating process is completed and the cooling process begins; the first stage of cooling adopts air cooling; when the surface temperature of the working layer of the roll drops to 650℃, the air cooling is changed to air cooling; when the surface temperature of the working layer of the high-speed steel roll drops to 480℃, the air cooling is stopped; Carry out the second air cooling; when the surface temperature of the working layer of the high-speed steel roll drops to 465°C, stop air cooling; the cooling process of the high-speed steel roll is completed.

9. A heat treatment method for increasing the service life of a high-speed steel roll according to claim 1, characterized in that: Step 4: When the high-speed steel roller is air-cooled to 420°C and the cooling process is completed, the high-speed steel roller is tempered; first, the high-speed steel roller is heated from 420°C to 480°C for 4 hours, and kept at 480°C for 6 hours; then the temperature is lowered, and after it drops to 250°C, it is heated to 520°C for 30 hours, and kept at 520°C for 10 hours; then the temperature is lowered, and it is kept at 100°C for 6 hours; then it is heated to 520°C for 42 hours, and kept at 520°C for 18 hours; then the temperature is lowered, and it is kept at 100°C for 6 hours, and then it is heated to 520°C for 42 hours, and kept at 520°C for 18 hours; then the temperature is lowered, and the surface of the working layer of the high-speed steel roller drops to 120°C and is taken out of the furnace, and the three temperings of the high-speed steel roller are completed.

10. A heat treatment method for increasing the service life of a high-speed steel roll according to claim 1, characterized in that: Step 1: The initial temperature in the high-speed steel roll chamber is 20°C. The furnace is heated to 140°C and the high-speed steel roll is placed in the furnace. The high-speed steel roll is first kept at 140°C for 5 hours. Then the high-speed steel roll is heated from 140°C to 570°C for 21 hours and kept at 570°C for 9 hours. Then the high-speed steel roll is heated from 570°C to 700°C for 7 hours and kept at 700°C for 13 hours to complete the preheating process of the high-speed steel roll. Step 2: Heat the high-speed steel roll from 700°C to 800°C for 5 hours, then heat from 800°C to 900°C for 21 hours, then heat from 900°C to 1030°C for 13 hours, keep warm at 1030°C for 7 hours, and complete the high-temperature section of the high-speed steel roll; Step 3: After the high-speed steel roll is kept at 1030℃ for 7 hours, the high-temperature heating process is completed and the cooling process begins; the first stage of cooling adopts air cooling; when the surface temperature of the working layer of the roll drops to 670℃, the air cooling is changed to air cooling; when the surface temperature of the working layer of the high-speed steel roll drops to 500℃, the air cooling is stopped; Carry out the second air cooling; when the surface temperature of the working layer of the high-speed steel roll drops to 470℃, stop air cooling; the cooling process of the high-speed steel roll is completed; Step 4: When the high-speed steel roller is air-cooled to 450°C and the cooling process is completed, the high-speed steel roller is tempered; first, the high-speed steel roller is heated from 450°C to 490°C for 5 hours, and kept at 490°C for 7 hours; then the temperature is lowered, and after it drops to 260°C, it is heated to 540°C for 31 hours, and kept at 540°C for 11 hours; then the temperature is lowered, and it is kept at 110°C for 7 hours; then it is heated to 540°C for 43 hours, and kept at 540°C for 19 hours; then the temperature is lowered, and it is kept at 110°C for 7 hours, and then it is heated to 540°C for 43 hours, and kept at 540°C for 19 hours; then the temperature is lowered, and the surface of the working layer of the high-speed steel roller drops to 130°C and is taken out of the furnace, and the three temperings of the high-speed steel roller are completed.

Citation Information

Cited By

  • Preparation method of wear-resistant high-speed steel plate strip roller

    CN120984854A