Method for synergistically utilizing red mud and refractory iron ore

Through the coordinated utilization of red mud and difficult-to-selected iron ore, including dehydration, granulation and suspension magnetization roasting, the problems of poor magnetic separation quality and prone to scar loss of red mud are solved, and the grade of iron concentrate is improved and Quality, achieving efficient iron resource recycling.

CN119040620APending Publication Date: 2024-11-29ZHENGZHOU NON FERROUS METALS RES INST CO LTD OF CHALCO
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411165803.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The quality of red mud is poor in magnetic iron separation concentrate and is prone to scarring and loss during the levitation magnetization roasting process.

Method used

By dehydrating and drying the red mud, mixing pretreatment products of difficult-to-select iron ore for granulation, suspending magnetization and water quenching, followed by wet grinding and weak magnetic separation to improve iron essence grade and quality of the ore.

Benefits of technology

It effectively solves the problem of scarring and fine-grained loss during the suspension magnetization roasting process of red mud, improves the grade and quality of iron concentrate, and realizes efficient recycling and utilization of iron resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040620A_ABST
    Figure CN119040620A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of comprehensive utilization of industrial solid wastes, in particular to a method for synergistically utilizing red mud and refractory iron ore. The method comprises the following steps: dehydrating red mud to obtain dehydrated red mud; drying and scattering the dehydrated red mud to obtain dry red mud; the method comprises the following steps: pretreating refractory iron ore to obtain rough iron concentrate, mixing the rough iron concentrate with dry red mud, and granulating and forming to obtain roasted raw material particles; drying the roasted raw material particles to obtain a dry raw material; carrying out suspension magnetization roasting on the dry raw material in a reducing atmosphere, and then carrying out water quenching to obtain a magnetization roasting clinker; the magnetized and roasted clinker is subjected to wet grinding and then subjected to low-intensity magnetic separation treatment, and iron ore concentrate is obtained; the diameter of the roasted raw material particles is 0.5 mm to 2.5 mm; the mass ratio of the dry red mud to the iron rough concentrate is (2: 8)-(6: 4). By means of the method, the technical problems that red mud and refractory iron ore scar and are prone to loss in suspension magnetization roasting can be solved, and the iron ore concentrate with the total iron content larger than or equal to 60.39% can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of comprehensive utilization of industrial solid wastes, and in particular to a method for coordinated utilization of red mud and refractory iron ore. Background Art

[0002] Red mud is a solid waste generated during the production of alumina. It is difficult to utilize due to its strong alkalinity, fine particle size, and complex properties. Therefore, it is currently generally treated by stockpiling. However, red mud is rich in iron, titanium, lithium, gallium, rare earths and other valuable metals. Therefore, the stockpiling of red mud will not only cause environmental pollution, but also secondary waste of resources. Although the reserves of iron ore resources are abundant at present, the endowment is too poor. Most of the iron ore resources are low-grade, complex and difficult-to-select ores (generally including limonite, siderite and / or oolitic hematite), which is difficult to meet the needs of the steel industry and social development. Therefore, the recovery of iron-containing minerals from high-iron red mud and limonite and siderite in iron ore resources can not only achieve the orderly reduction and resource utilization of red mud solid waste, but also promote the healthy and high-quality development of the alumina industry. At present, the iron-containing minerals in the high-iron red mud are mainly present in the form of aluminum goethite and hematite, but the magnetism of aluminum goethite is weak, which leads to poor iron selection index of direct magnetic separation or re-selection of red mud, and it is difficult to obtain high-quality iron concentrate with low impurity content (TFe content>56%) from red mud. For example, the iron concentrate obtained by direct magnetic separation of red mud dissolved from Guinea ore has poor quality (TFe content<50%). In addition, as a potential raw material for steel, difficult-to-select iron minerals have the disadvantages of complex genesis, relatively weak magnetism, uneven particle size, and easy mudification during grinding, which increases the difficulty of beneficiation of difficult-to-select iron minerals; in addition, some difficult-to-select iron ores are also rich in crystal water and have a low theoretical grade of TFe. It is difficult to reach a grade of 60% for the iron ore concentrate extracted by conventional physical beneficiation methods alone.

[0003] Although it is currently possible to use suspended magnetization roasting to recycle iron-containing resources from high-iron red mud and refractory iron ore, the principle is to magnetize and modify the weakly magnetic iron minerals in high-iron red mud and refractory iron ore to improve their magnetic properties, and then perform weak magnetic separation of iron after magnetization modification. However, the suspended magnetization roasting method still has the defects of high viscosity of high-iron red mud, high moisture content of filter cake, high energy consumption of drying, and poor fluidity of red mud. In addition, there are defects such as dissolution scarring, easy damage to fine particles, and high impurity content of iron concentrate in the direct suspended magnetization roasting process. In addition, the refractory iron ore in the direct suspended magnetization roasting process has problems such as fine particle size, easy mudification, easy scarring during roasting, and easy loss of fine particles. These problems will lead to poor grade of the final iron concentrate.

[0004] The existing technologies for recycling iron-containing resources from high-iron red mud and refractory iron ore by suspended magnetic roasting include: (1) a process for producing iron concentrate by suspended magnetic roasting and then grinding red mud, wherein the process flow is as follows: drying the iron-containing red mud to obtain dry red mud, and then crushing and mixing the dry red mud with additives to obtain a mixed material; then adding the mixed material to a suspended heating furnace for reduction reaction, controlling the reduction time to be 15s to 25s, and the terminal temperature of the reduction to be 800°C to 900°C, and then performing suspended magnetic roasting to obtain a high-temperature roasted material; the high-temperature roasted material is finally cooled by an oxygen-free cooling device and wet ground, and then subjected to magnetic separation by a two-stage magnetic separator to obtain a higher-grade iron concentrate. (2) A method for producing iron concentrate by using refractory limonite for staged roasting, grinding and magnetic separation, wherein the process flow is as follows: first, the refractory limonite is ground to obtain limonite powder, and then the limonite powder is sent into a three-stage suspension roasting system by a cyclone to promote the oxidation reaction of the limonite powder with air in a suspended state, and then the limonite powder is sent into a cooler after staged suspension roasting, and discharged to air cool after the temperature drops to 200-300°C to obtain roasted material; the roasted material is ground and then subjected to three-stage magnetic separation to obtain iron concentrate and tailings. (3) A method for beneficiating refractory iron ore using high carbonate, the process flow of which is: first, subject the iron ore to X-ray transmission to pre-selection to obtain a pre-selected concentrate and pre-selected tailings rich in siderite; then, subject the pre-selected concentrate rich in siderite to magnetization roasting and grinding weak magnetic separation to obtain a roasted magnetic concentrate and a roasted magnetic tailings; then, subject the pre-selected tailings to grinding and then strong magnetic separation to obtain a strong magnetic concentrate and a strong magnetic tailings; then, subject the strong magnetic concentrate to reverse flotation to obtain a reverse flotation concentrate and a reverse flotation tailings. Summary of the invention

[0005] The present application provides a method for the coordinated utilization of red mud and refractory iron ore to solve the following technical problems: how to solve the problem that the quality of iron concentrate obtained by magnetic separation of red mud alone is poor, and the fine particles of red mud and refractory iron ore are prone to scarring and loss during suspended magnetic roasting.

[0006] In a first aspect, the present application provides a method for the coordinated utilization of red mud and refractory iron ore, the method comprising:

[0007] Dehydrating the red mud to obtain dehydrated red mud;

[0008] Drying and breaking up the dehydrated red mud to obtain dry red mud;

[0009] Pre-treating refractory iron ore to obtain rough iron concentrate;

[0010] The crude iron concentrate and the dry red mud are mixed, and then granulated to obtain roasted raw material particles;

[0011] Drying the roasted raw meal particles to obtain dry raw meal;

[0012] The dry raw material is subjected to suspended magnetization roasting in a reducing atmosphere, and then water quenching to obtain magnetization roasted clinker;

[0013] The magnetized roasted clinker is wet-grinded and then weakly magnetically separated to obtain an iron concentrate; wherein the weight ratio of the granular material with a particle size of less than 0.023 mm in the red mud to the red mud is 0.4 to 0.8;

[0014] The diameter of the roasted raw material particles is 0.5 mm to 2.5 mm;

[0015] The mass ratio of the dry red mud to the rough iron concentrate is 2:8 to 6:4.

[0016] Optionally, the ratio of the total iron content of the red mud to the total weight of the red mud is ≥0.3;

[0017] The ratio of the total iron content of the refractory iron ore to the total weight of the refractory iron ore is ≥0.25, and the refractory iron ore includes at least one of the following:

[0018] Refractory limonite, refractory siderite and refractory oolitic hematite.

[0019] Optionally, the moisture content of the dehydrated red mud is ≤21%;

[0020] The moisture content of the dry red mud is 7% to 14%;

[0021] The moisture content of the dry raw material is 4% to 7.5%.

[0022] Optionally, the drying medium used for the drying is the roasting tail gas of the suspended magnetization roasting;

[0023] The drying medium used in the drying is the drying tail gas from the drying.

[0024] Optionally, the reducing atmosphere includes a carbon monoxide atmosphere, and the carbon monoxide volume concentration of the carbon monoxide atmosphere is 3.5% to 5.5%;

[0025] The temperature of the suspended magnetization roasting is 500° C. to 900° C., and the time of the suspended magnetization roasting is 0.5 min to 3.5 min.

[0026] Optionally, the terminal grinding fineness of the wet grinding satisfies: the mass ratio of the first fine-grained material to the magnetized roasted clinker is 60% to 75%; wherein the particle size of the first fine-grained material is ≤0.038 mm.

[0027] Optionally, the weak magnetic separation process includes weak magnetic roughing and weak magnetic fine separation, the magnetic field strength of the weak magnetic roughing is 0.3T to 0.5T, and the magnetic field strength of the weak magnetic fine separation is 0.1T to 0.3T.

[0028] Optionally, the pretreatment includes crushing, dry grinding and dry magnetic separation; wherein, the terminal grinding fineness of the dry grinding satisfies: the mass ratio of the second fine-grained material to the difficult-to-select iron ore is 60% to 85%; wherein, the particle size of the second fine-grained material is ≤0.038mm.

[0029] Optionally, the dry magnetic separation process includes dry roughing and dry sweeping, the magnetic field strength of the dry roughing is 0.5T to 0.9T, and the magnetic field strength of the dry sweeping is 1.0T to 1.3T.

[0030] Optionally, the total iron content of the iron concentrate is ≥60%, the total content of sodium oxide and potassium oxide of the iron concentrate is ≤0.20%, the aluminum oxide content of the iron concentrate is ≤2.0%, and the titanium oxide content of the iron concentrate is ≤0.35%.

[0031] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0032] The present application provides a method for the coordinated utilization of red mud and refractory iron ore, the method comprising:

[0033] The red mud is dehydrated to obtain dehydrated red mud; the dehydrated red mud is dried and broken up to obtain dry red mud; the refractory iron ore is pretreated to obtain a rough iron concentrate; the rough iron concentrate and the dry red mud are mixed and then granulated to obtain roasted raw material particles; the roasted raw material particles are dried to obtain dry raw material; the dry raw material is suspended magnetized roasted in a reducing atmosphere and then water quenched to obtain magnetized roasted clinker; the magnetized roasted clinker is wet ground and then weakly magnetically separated to obtain iron concentrate; wherein the weight ratio of the granular material with a particle size of less than 0.023 mm in the red mud to the red mud is 0.4-0.8; the diameter of the roasted raw material particles is 0.5 mm-2.5 mm; the ratio of the dry red mud to the rough iron concentrate is 2:8-6:4. The weight ratio of the particulate material with a particle size of less than 0.023 mm in the red mud to the red mud can be 0.4-0.8, and the diameter of the roasted raw material particles can be 0.5 mm-2.5 mm, which can indicate that the particle size of the red mud is fine. The use of the rough iron concentrate can not only adjust the mineral components and elemental composition of the dry red mud, but also act as a water absorbent to adjust the moisture of the dry red mud to obtain the roasted raw material particles with uniform component distribution and dryness. In addition, the particle size of the roasted raw material particles formed by the dry red mud and the fine-grained refractory iron ore can be increased by granulating the rough iron concentrate with the dry red mud, thereby improving the fluidity of the roasted raw material particles; in addition, the mass ratio of the dry red mud to the rough iron concentrate is generally 2:8-6:4, which can promote the formation of a uniform roasted raw material between the dry red mud and the rough iron concentrate. Raw material particles, roasted raw material particles with uniform composition can effectively remove moisture during the drying stage to obtain fully dried, low-impurity, and high-fluidity roasted raw material particles. The high-fluidity roasted raw material particles can solve the technical problems of scarring and easy loss of fine-grained materials due to poor fluidity during suspended magnetic roasting in the subsequent suspended magnetic roasting process, and can further promote the directional transformation of weakly magnetic iron minerals in the iron-containing minerals of the roasted raw material particles to strongly magnetic iron minerals, so as to achieve the mineral phase reconstruction reaction of the iron-containing minerals in the roasted raw material particles, thereby obtaining magnetic roasted clinker with a high content of strongly magnetic iron minerals. The magnetic roasted clinker with a high content of strongly magnetic iron minerals can be screened out into iron concentrate products with higher grade and less impurity content through wet grinding and weak magnetic separation. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0035] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0036] Figure 1 A schematic flow chart of a method for coordinated utilization of red mud and refractory iron ore provided in an embodiment of the present application;

[0037] Figure 2 A schematic diagram of the actual process flow of a method for the coordinated utilization of red mud and refractory iron ore provided in an embodiment of the present application. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0039] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a rigid limitation on the scope of the present application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within the range; for example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range; in addition, whenever a numerical range is indicated in this document, it is meant to include any cited numbers (fractions or integers) within the indicated range.

[0040] In this document, the terms including "including" and "including" mean "including but not limited to". Relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. "And / or" describes the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone; where A and B can be singular or plural. "At least one" means one or more, and "plurality" means two or more; "at least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items; for example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple. Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0041] It should be noted that, with respect to the prior art (1) recorded in the background technology, the inventors found that: the process also has the problems of high red mud drying cost, scarring during suspended magnetized roasting, serious loss of red mud fine-grained grade, and high impurity content in iron ore concentrate; with respect to the prior art (2) recorded in the background technology, the inventors found that: during the suspended roasting process, the inventors found that: the process has the problems of scarring during dehydration of limonite, loss of fine-grained limonite, and low TFe content in tailings and iron ore concentrate; with respect to the prior art (3) recorded in the background technology, the inventors found that: during the magnetized roasting process, the inventors found that: siderite decomposition occurs in the process, which easily leads to production problems of easy pulverization and scarring of iron ore.

[0042] Figure 1 A schematic flow chart of a method for coordinated utilization of red mud and refractory iron ore provided in an embodiment of the present application is exemplarily shown;

[0043] like Figure 1 As shown, the embodiment of the present application provides a method for the coordinated utilization of red mud and refractory iron ore, the method comprising:

[0044] S1. dehydrating the red mud to obtain dehydrated red mud;

[0045] S2. drying and breaking up the dehydrated red mud to obtain dry red mud;

[0046] S3. Pre-treating the refractory iron ore to obtain a rough iron concentrate;

[0047] S4. The crude iron concentrate and the dry red mud are mixed, and then granulated to obtain roasted raw material particles;

[0048] S5. Drying the roasted raw material particles to obtain dry raw material;

[0049] S6. The dry raw material is subjected to suspended magnetization roasting in a reducing atmosphere, and then water quenched to obtain magnetized roasted clinker;

[0050] S7. The magnetized roasted clinker is wet ground and then subjected to weak magnetic separation to obtain an iron concentrate;

[0051] Wherein, the weight of the granular material with a particle size of less than 0.023 mm in the red mud and the red mud is 0.4 to 0.8;

[0052] The diameter of the roasted raw material particles is 0.5 mm to 2.5 mm;

[0053] The mass ratio of the dry red mud to the rough iron concentrate is 2:8 to 6:4;

[0054] In these embodiments, the mass ratio of dry red mud to rough iron concentrate can be 2:8 to 6:4. On the one hand, rough iron concentrate can be added to dry red mud to adjust the elemental composition and phase composition of the roasted raw material particles. On the other hand, rough iron concentrate can be used as a water absorbent to adjust the moisture content of the dry red mud to obtain roasted raw material particles with uniform component distribution and dryness. The roasted raw material particles with uniform component distribution and dryness can effectively solve the technical problems of easy scarring and easy loss of fine particles during the suspended magnetic roasting of high red mud and difficult-to-select iron ore in the subsequent drying stage, so as to obtain a fully dried dry material with a low impurity content. The fully dried dry material with a low impurity content can further promote the weak magnetic iron ore in the iron-containing minerals of the dry material in the subsequent suspended magnetic roasting process. The dry material undergoes a directional transformation into strongly magnetic iron minerals to achieve a mineral phase reconstruction reaction of the iron-containing minerals in the dry material, thereby obtaining a magnetized roasted clinker with a high content of strongly magnetic iron minerals. The magnetized roasted clinker with a high content of strongly magnetic iron minerals can be screened out into an iron concentrate product with a higher grade and less impurities through wet grinding and weak magnetic separation. If the mass ratio of dry red mud to iron coarse concentrate is less than 2:8, it will be difficult to achieve the purpose of large-scale and resource-based disposal of red mud due to the small amount of dry red mud used. If the mass ratio of dry red mud to iron coarse concentrate is greater than 6:4, the content of iron coarse concentrate is too little, and it will not be able to reduce the moisture content of the mixed material and adjust the elemental composition and phase composition of the roasted raw material particles, resulting in a decrease in the quality of the iron concentrate.

[0055] In addition, the weight ratio of particulate material with a particle size of less than 0.023 mm in the red mud to red mud can be 0.4-0.8, and the diameter of the roasted raw material particles can be 0.5 mm-2.5 mm, which can explain that the particle size composition of the red mud is fine, and the iron coarse concentrate and the dry red mud are fully mixed. The iron coarse concentrate can be used to adjust the mineral composition of the red mud and granulate the red mud and the iron coarse concentrate, so as to increase the particle size of the dry red mud through the large particle size of the iron coarse concentrate, thereby improving the fluidity of the roasted raw material particles.

[0056] The mass ratio of the dry red mud to the rough iron concentrate may be 2:8, 3:7, 4:6, 5:5 or 6:4.

[0057] The weight ratio of the particulate material with a particle size of less than 0.023 mm in the red mud to the red mud can be 0.40, 0.45, 0.50, 0.55, 0.60, 0.65, 0.70, 0.75 or 0.80.

[0058] The diameter of the calcined raw material particles can be 0.5mm, 0.6mm, 0.7mm, 0.8mm, 0.9mm, 1.0mm, 1.1mm, 1.2mm, 1.3mm, 1.4mm, 1.5mm, 1.6mm, 1.7mm, 1.8mm, 1.9mm, 2.0mm, 2.1mm, 2.2mm, 2.3mm, 2.4mm or 2.5mm.

[0059] It should be noted that the total iron content of the red mud can be 30% or more, and the total iron content of the refractory iron ore can be 25% or more.

[0060] It should be noted that the red mud can be raw red mud or concentrate obtained by strong magnetic separation of raw red mud.

[0061] It should be noted that the pretreatment can also obtain the first tailings, and the weak magnetic separation treatment can also obtain the second tailings. The first tailings and the second tailings can be combined and processed to obtain tailings products, and these tailings products can be sold as raw materials for preparing cement or raw materials for preparing concrete to realize the material utilization of tailings, thereby improving the comprehensive utilization rate of tailings and realizing the full quantitative utilization of red mud and difficult-to-select iron ore.

[0062] In some optional embodiments, the ratio of the total iron content of the red mud to the total weight of the red mud is ≥0.3;

[0063] The ratio of the total iron content of the refractory iron ore to the total weight of the refractory iron ore is ≥0.25, and the refractory iron ore includes at least one of the following:

[0064] Refractory limonite, refractory siderite and refractory oolitic hematite;

[0065] In these embodiments, the ratio of the total iron content of red mud to the total weight of red mud can be ≥0.3, and the ratio of the total iron content of refractory iron ore to the total weight of refractory iron ore can be ≥0.25, so as to ensure that there is sufficient iron in red mud and refractory iron ore, and the sufficient iron can define the raw material selection range for red mud and refractory iron ore, and iron concentrate products with better TFe grade and lower impurity content can be obtained in subsequent methods, so as to improve the feasibility and reliability of the method of the embodiment of the present application; in addition, the refractory iron ore can include at least one of refractory limonite, refractory siderite and refractory oolitic hematite, which can make the refractory iron ore cover most of the refractory iron ore with higher total iron content, so as to make the total iron content of the refractory iron ore 25% or above.

[0066] In some optional embodiments, the moisture content of the dehydrated red mud is ≤21%;

[0067] The moisture content of the dry red mud is 7% to 14%;

[0068] The moisture content of the dry raw material is 4% to 7.5%;

[0069] In these embodiments, the moisture content of the dehydrated red mud can be ≤21%, and the moisture of the red mud can be removed as much as possible by dehydration treatment to reduce the moisture content of the red mud. On the one hand, the dehydration treatment with low moisture content can facilitate the subsequent use of the roasting tail gas of the suspended roasting to dry the dehydrated treatment, and on the other hand, the dehydration treatment with low moisture content can provide the dry raw material with process conditions that are conducive to suspended magnetization roasting; in addition, the moisture content of the dry red mud can be 7% to 14%, indicating that the drying and breaking effects are good, so as to facilitate the subsequent mixing operation of the rough iron concentrate and the dry red mud; in addition, the dry raw material The moisture content can be 4% to 7.5%, which can keep the moisture content of the dry raw material at a lower level to improve the fluidity of the dry raw material and avoid the adhesion of the roasted raw material particles in the subsequent suspended magnetized roasting stage, thereby improving the magnetization effect of the iron coarse concentrate and dry red mud in the subsequent suspended magnetized roasting stage to achieve the mineral phase reconstruction reaction of the iron-containing minerals in the dry material, and then obtain the magnetized roasted clinker with a high content of strongly magnetic iron minerals. The magnetized roasted clinker with a high content of strongly magnetic iron minerals can be screened out into iron concentrate products with high TFe grade and low impurity content through wet grinding and weak magnetic separation.

[0070] The moisture content of the dried red mud may be 7%, 8%, 9%, 10%, 11%, 12%, 13% or 14%.

[0071] The moisture content of the dry raw meal can be 4.0%, 4.5%, 5.0%, 5.5%, 6.0%, 6.5%, 7.0% or 7.5%.

[0072] It should be noted that when the moisture content of dry red mud is lower than 7%, the energy consumption of drying will increase, which means that in addition to the roasting exhaust gas of suspended magnetic roasting, new drying medium needs to be introduced as the drying medium used for drying, thereby increasing the overall cost of drying; and when the moisture content of dry red mud exceeds 14%, the dry red mud will be agglomerated to form floc particles, and the dry red mud containing floc particles will be difficult to mix fully with the rough iron concentrate, thereby increasing the difficulty of suspended magnetic roasting.

[0073] It should be noted that when the moisture content of the dry raw material is lower than 4.0%, the energy consumption of drying will increase, which will result in the need to introduce new drying medium in addition to the drying exhaust gas used for drying, thereby increasing the overall cost of drying; and when the moisture content of the dry raw material exceeds 7.5%, it will cause the particles of the roasted raw material particles to stick together and reduce the fluidity of the dry raw material, and the low fluidity of the dry raw material will increase the difficulty of suspended magnetization roasting.

[0074] In some optional embodiments, the drying medium used for the drying is the roasting tail gas of the suspended magnetization roasting;

[0075] The drying medium used in the drying is the drying tail gas from the drying;

[0076] In these embodiments, the drying medium used for drying generally uses the roasting tail gas of suspended magnetic roasting, and the roasting tail gas of suspended magnetic roasting can be used as the drying medium for dehydrated red mud to dry the dehydrated red mud into dry red mud, so that the moisture in the red mud can be fully removed, so as to facilitate the subsequent mixing of dry red mud and iron coarse concentrate and the preparation of raw material particles; in addition, the drying medium used for drying generally uses the drying tail gas of drying, and the tail gas generated by drying the dehydrated red mud can be used as the drying medium for roasting raw material particles to dry the roasted raw material particles into dry raw material, so that the moisture in the roasted raw material particles can be fully removed, so as to improve the fluidity of the dry raw material and thus solve the problem of scarring and easy loss of red mud and fine particles of refractory iron ore during suspended magnetic roasting.

[0077] In some optional embodiments, the reducing atmosphere comprises a carbon monoxide atmosphere, and the carbon monoxide volume concentration of the carbon monoxide atmosphere is 3.5% to 5.5%;

[0078] The temperature of the suspended magnetization roasting is 500° C. to 900° C., and the time of the suspended magnetization roasting is 0.5 min to 3.5 min.

[0079] In these embodiments, the reducing atmosphere may include a carbon monoxide atmosphere, and the carbon monoxide volume concentration of the carbon monoxide atmosphere may be 3.5% to 5.5%, which can promote the presence of sufficient reducing gas during the suspended magnetic roasting process. The sufficient reducing gas can promote the directional transformation of weakly magnetic iron minerals in the dry material into strongly magnetic iron minerals, so as to achieve the mineral phase reconstruction reaction of the iron-containing minerals in the dry material, thereby obtaining a magnetic roasted clinker with a high content of strongly magnetic iron minerals; in addition, the temperature of the suspended magnetic roasting can be 500°C to 900°C, and the time of the suspended magnetic roasting can be 0.5min to 3.5min, which can promote the directional transformation of weakly magnetic iron minerals in the dry material into strongly magnetic iron minerals during the suspended magnetic roasting process, so as to achieve the mineral phase reconstruction reaction of the iron-containing minerals in the dry material, thereby obtaining a magnetic roasted clinker with a high content of strongly magnetic iron minerals.

[0080] The carbon monoxide volume concentration of the carbon monoxide atmosphere can be 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5.0%, 5.1%, 5.2%, 5.3%, 5.4% or 5.5%.

[0081] The temperature of the suspended magnetization roasting can be 500℃, 510℃, 520℃, 530℃, 540℃, 550℃, 560℃, 570℃, 580℃, 590℃, 600℃, 610℃, 620℃, 630℃, 640℃, 650℃, 660℃, 670℃, 680℃, 690℃, 700℃, 710℃, 720℃, 730℃, 740℃, 750℃, 760℃, 770℃, 780℃, 790℃, 800℃, 810℃, 820℃, 830℃, 840℃, 850℃, 860℃, 870℃, 880℃, 890℃ or 900℃.

[0082] The time of the suspended magnetization calcination can be 0.5min, 0.6min, 0.7min, 0.8min, 0.9min, 1.0min, 1.1min, 1.2min, 1.3min, 1.4min, 1.5min, 1.6min, 1.7min, 1.8min, 1.9min, 2.0min, 2.1min, 2.2min, 2.3min, 2.4min, 2.5min, 2.6min, 2.7min, 2.8min, 2.9min, 3.0min, 3.1min, 3.2min, 3.3min, 3.4min or 3.5min.

[0083] It should be noted that when the volume concentration of carbon monoxide in the carbon monoxide atmosphere is lower than 3.5%, it will lead to insufficient directional conversion of weakly magnetic iron-containing minerals such as alnicotinite and hematite in the dry raw material into strongly magnetic iron minerals, thereby affecting the iron index of the subsequent weak magnetic separation treatment. When the volume concentration of carbon monoxide in the carbon monoxide atmosphere exceeds 5.5%, the above will cause excessive CO in the reducing gas. Excessive CO will continue to undergo redox reactions with the magnetite generated by suspended magnetic roasting to generate weakly magnetic FeO and other minerals, thereby reducing the subsequent recovery rate of iron concentrate.

[0084] It should be noted that when the temperature of the suspended magnetic roasting is lower than 500°C, the mineral phase reconstruction reaction of the iron-containing matter in the dry raw material will not be complete during the suspended magnetic roasting process, which will affect the conversion rate of weakly magnetic iron-containing minerals such as alnicotinite and hematite in the dry raw material to magnetite. When the temperature of the suspended magnetic roasting exceeds 900°C, the generated strong magnetic magnetite will be over-reduced, that is, Fe3O4 will continue to react with CO to generate FeO and Fe with relatively weak magnetic properties, resulting in the loss of part of the iron-containing minerals in the dry raw material in the tailings, thereby causing the iron concentrate indicators of the weak magnetic separation treatment to deteriorate. In addition, the production cost of the suspended magnetic roasting will be increased.

[0085] It should be noted that when the suspended magnetic roasting time is less than 0.5 min, the suspended magnetic roasting time will be insufficient, which will lead to incomplete reaction of weakly magnetic iron minerals such as alnicotinite and hematite in the dry raw material into strongly magnetic magnetite, resulting in some weakly magnetic iron minerals being lost in the tailings and affecting the iron index of weak magnetic separation treatment; when the suspended magnetic roasting time exceeds 3.5 min, the already transformed strongly magnetic magnetite (Fe3O4) will continue to react with CO to generate FeO with relatively weak magnetism, which will lead to a decrease in the recovery rate of iron concentrate after weak magnetic separation treatment. In addition, a long time of magnetic roasting time will cause problems such as increased production costs and reduced production efficiency.

[0086] In some optional embodiments, the terminal grinding fineness of the wet grinding satisfies: the mass ratio of the first fine-grained material to the magnetized roasted clinker is 60% to 75%; wherein the particle size of the first fine-grained material is ≤0.038 mm;

[0087] In these embodiments, the terminal grinding fineness of wet grinding can meet the following requirements: the mass ratio of the first fine-grained material to the magnetized roasted clinker can be 60% to 75%, and the particle size of the first fine-grained material is generally ≤0.038 mm, which can promote the monomer dissociation of iron-containing minerals and other gangue minerals in the roasted clinker as much as possible, so as to facilitate the subsequent weak magnetic separation treatment process.

[0088] The mass ratio of the first fine-grained material to the magnetized roasted clinker can be 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74% or 75%.

[0089] It should be noted that when the mass ratio of the first fine-grained material to the magnetized roasted clinker is lower than 60%, the dissociation effect of the iron-containing minerals and other gangue mineral monomers of the magnetized roasted clinker will be poor, resulting in the subsequent weak magnetic separation treatment being unable to obtain qualified iron concentrate; when the mass ratio of the first fine-grained material to the magnetized roasted clinker is higher than 75%, the iron-containing minerals of the magnetized roasted clinker will be excessively worn and lost in the tailings, thereby reducing the TFe recovery rate of the iron concentrate and increasing the grinding energy consumption.

[0090] In some optional embodiments, the weak magnetic separation process includes weak magnetic roughing and weak magnetic concentrating, the magnetic field strength of the weak magnetic roughing is 0.3T to 0.5T, and the magnetic field strength of the weak magnetic concentrating is 0.1T to 0.3T;

[0091] In these embodiments, weak magnetic separation treatment may include weak magnetic roughing and weak magnetic concentration, and the magnetic field strength of the weak magnetic roughing may be 0.3T to 0.5T, and the magnetic field strength of the weak magnetic concentration may be 0.1T to 0.3T, which is beneficial for screening out iron concentrate products with higher TFe content and lower impurity content from the magnetized roasted clinker after wet grinding, and can ensure the recovery rate of iron concentrate products treated with weak magnetic separation of the magnetized roasted clinker, thereby obtaining excellent weak magnetic separation indicators.

[0092] The magnetic field strength of the weak magnetic roughing can be 0.3T, 0.4T or 0.5T.

[0093] The magnetic field strength of the weak magnetic concentration can be 0.1T, 0.2T or 0.3T.

[0094] It should be noted that when the magnetic field intensity of the weak magnetic roughing is lower than 0.3T, although the total iron content of the iron concentrate after weak magnetic separation treatment will be increased to obtain high-grade iron concentrate, the recovery rate of the iron concentrate treated with weak magnetic separation is low; when the magnetic field intensity of the weak magnetic roughing exceeds 0.5T, it will lead to serious mechanical inclusions during the weak magnetic separation process, thereby greatly reducing the total iron content of the iron concentrate after weak magnetic separation treatment, and further affecting the magnetic separation effect of the weak magnetic separation treatment.

[0095] It should be noted that when the magnetic field strength of the weak magnetic concentration is lower than 0.1 T, the magnetic field strength of the weak magnetic concentration will be reduced, and a relatively weak magnetic field strength of the weak magnetic concentration will reduce the yield of the iron concentrate; when the value of the concentration magnetic field strength is too large, the TFe content of the iron concentrate will be reduced and the quality of the iron concentrate will be affected.

[0096] In some optional embodiments, the pretreatment includes crushing, dry grinding and dry magnetic separation; wherein the terminal grinding fineness of the dry grinding satisfies: the mass ratio of the second fine-grained material to the refractory iron ore is 60% to 85%; wherein the particle size of the second fine-grained material is ≤0.038 mm;

[0097] In these embodiments, pretreatment may include crushing, dry grinding and dry magnetic separation, and the terminal grinding fineness of dry grinding may satisfy: the mass ratio of the second fine particle size material to the refractory iron ore may be 60% to 85%, and dry grinding may be used to achieve monomer dissociation of iron-containing minerals and other minerals in the refractory iron ore, so as to ultimately make the particle size of most of the iron coarse concentrate below 0.038 mm, so as to facilitate the subsequent use of the iron coarse concentrate to increase the particle size of the dry red mud, so as to avoid the subsequent scarring of the roasted raw material particles in the suspended magnetic roasting stage; in addition, the selection method of dry grinding can facilitate the acquisition of iron coarse concentrate, which is beneficial to the subsequent reduction of the moisture content of the roasted raw material particles to save drying costs.

[0098] The mass ratio of the second fine-grained material to the refractory iron ore can be 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84% or 85%.

[0099] It should be noted that when the mass ratio of the second fine-grained material to the refractory iron ore is lower than 60%, the dissociation effect of the iron-containing minerals in the refractory iron ore from other mineral monomers will be poor, which will lead to excessively high impurity content in the iron concentrate after dry magnetic separation and reduce the total iron content of the iron concentrate; when the mass ratio of the second fine-grained material to the refractory iron ore is higher than 85%, the iron-containing minerals in the refractory iron ore will be excessively worn and lost in the first tailings, thereby reducing the total iron recovery rate in the obtained iron concentrate.

[0100] In some optional embodiments, the dry magnetic separation process includes dry roughing and dry sweeping, the magnetic field strength of the dry roughing is 0.5T to 0.9T, and the magnetic field strength of the dry sweeping is 1.0T to 1.3T;

[0101] In these embodiments, the dry magnetic separation treatment may include dry roughing and dry scavenging, and the magnetic field intensity of the dry roughing may be 0.5T to 0.9T, and the magnetic field intensity of the dry scavenging may be 1.0T to 1.3T, which is not only beneficial to increase the total iron content in the iron rough concentrate obtained by the dry magnetic separation treatment, but also to increase the total iron recovery rate in the iron rough concentrate after the dry magnetic separation treatment, thereby obtaining an iron rough concentrate with excellent iron selection indicators.

[0102] The magnetic field strength of the dry roughing can be 0.5T, 0.6T, 0.7T, 0.8T or 0.9T.

[0103] The magnetic field strength of the dry scanning can be 1.0T, 1.1T, 1.2T or 1.3T.

[0104] It should be noted that when the magnetic field intensity of the dry roughing is lower than 0.5T, although the total iron grade of the iron rough concentrate will be increased, the yield of the iron rough concentrate will be reduced; when the magnetic field intensity of the dry roughing exceeds 0.9T, the degree of mechanical inclusions in the dry roughing process will be increased, thereby significantly reducing the total iron content of the iron rough concentrate after dry magnetic separation, thereby affecting the effect of the dry magnetic separation treatment.

[0105] When the magnetic field intensity of the dry sweeping is lower than 1.0T, the magnetic field intensity of the dry sweeping will be reduced, and the weak dry sweeping magnetic field intensity cannot effectively obtain the swept concentrate; when the magnetic field intensity of the dry sweeping exceeds 1.3T, it will not only reduce the total iron content in the rough iron concentrate screened out by the dry sweeping magnetic field, but also increase the additional energy consumption of the dry sweeping, thereby increasing the production cost of the dry sweeping.

[0106] In some optional embodiments, the total iron content of the iron concentrate is ≥60%, the total content of sodium oxide and potassium oxide of the iron concentrate is ≤0.20%, the aluminum oxide content of the iron concentrate is ≤2.0%, and the titanium oxide content of the iron concentrate is ≤0.35%;

[0107] In these embodiments, the total iron content of the iron concentrate is generally ≥60%, and the total content of sodium oxide and potassium oxide in the iron concentrate is generally ≤0.20%, and the aluminum oxide content of the iron concentrate is generally ≤2.0%, and the titanium oxide content of the iron concentrate is generally ≤0.35%, which means that the iron concentrate extracted by the method provided in the embodiment of the present application contains sufficient iron elements and less harmful impurities (Na2O, K2O, Al2O3 and TiO2), which can meet the requirements of C60 in the national quality standard for iron concentrate GB / T36704-2018, so as to achieve the quality standard of iron concentrate for ironmaking.

[0108] The present application is further described below in conjunction with specific examples. The experimental methods in the following examples that do not specify specific conditions are usually measured according to industry standards; if there are no corresponding industry standards, they are carried out according to common international standards, conventional conditions, or conditions recommended by the manufacturer.

[0109] Example 1

[0110] High-iron red mud and refractory limonite from a certain place in Henan Province were selected. The chemical composition of the high-iron red mud met the following requirements: Al2O3: 17.88%, SiO2: 11.93%, TFe: 38.35% by mass fraction. In addition, the iron-containing minerals in the high-iron red mud are mainly alumina goethite and red mud ore, wherein the mass ratio of alumina goethite to iron-containing minerals is 0.5675. The high-iron red mud also contains other gangue minerals, including sodium silicate slag, rutile, anatase, gibbsite and a small amount of diaspore.

[0111] Refractory iron ore is refractory limonite. In terms of mass fraction, the main chemical components of refractory limonite meet the following requirements: TFe: 36.81%, Al2O3: 1.98%, SiO2: 12.93%. In addition, limonite is the main iron-bearing mineral in refractory limonite, and the rest are gangue minerals, which are mainly dolomite, calcite and a small amount of quartz.

[0112] like Figure 1 and Figure 2 As shown, a method for synergistic utilization of red mud and refractory iron ore comprises the steps of:

[0113] S1. Using an ultra-high pressure filter press to dehydrate the red mud mainly by filter pressing dehydration to obtain dehydrated red mud and filtrate; wherein the filtrate can be comprehensively recycled;

[0114] S2. drying and breaking up the dehydrated red mud using the roasting tail gas of the suspended magnetized roasting furnace to obtain dry red mud and drying tail gas, respectively;

[0115] S3. crushing, dry grinding and dry magnetic separation of the refractory iron ore to obtain a rough iron concentrate and a first tailings;

[0116] S4. The crude iron concentrate and the dry red mud are mixed, and then granulated using a granulator to obtain roasted raw material particles;

[0117] S5. Drying the roasted raw meal particles using drying exhaust gas to obtain dry raw meal;

[0118] S6. The dry raw material is subjected to suspended magnetization roasting in a reducing atmosphere, and then rapidly cooled by water quenching to obtain magnetized roasted clinker;

[0119] S7. Wet grinding the magnetized roasted clinker, and then performing weak magnetic separation to obtain iron concentrate and second tailings, respectively;

[0120] S8. merging the first tailings and the second tailings to obtain tailings;

[0121] The mass ratio of dry red mud to rough iron concentrate is 50:50.

[0122] The moisture content of dehydrated red mud is 20.58%;

[0123] The moisture content of dry red mud is 13.22%;

[0124] The moisture content of the dry raw meal is 6.12%.

[0125] The diameter of the roasted raw material particles is 1.0 mm.

[0126] The reducing atmosphere includes a carbon monoxide atmosphere, and the carbon monoxide volume concentration of the carbon monoxide atmosphere is 3.50%;

[0127] The temperature of suspended magnetization roasting is 690°C, and the time of suspended magnetization roasting is 2.5min.

[0128] The terminal grinding fineness of wet grinding satisfies: the mass ratio of the first fine-grained material to the magnetized roasted clinker is 63.47%; wherein the particle size of the first fine-grained material is ≤0.038 mm.

[0129] The weak magnetic separation process includes weak magnetic roughing and weak magnetic concentrating. The magnetic field strength of the weak magnetic roughing is 0.35T, and the magnetic field strength of the weak magnetic concentrating is 0.25T.

[0130] The pretreatment includes crushing, dry grinding and dry magnetic separation. The terminal grinding fineness of dry grinding satisfies that the mass ratio of the second fine particle size material to the refractory iron ore is 64.52%. The particle size of the second fine particle size material is ≤0.038mm.

[0131] Dry magnetic separation treatment includes dry roughing and dry scavenging. The magnetic field strength of dry roughing is 0.7T, and the magnetic field strength of dry scavenging is 1.2T.

[0132] The product parameters of the iron ore concentrate, the first tailings, the iron ore concentrate, the second tailings and the roasted raw material particles obtained in each step are shown in Table 1.

[0133] Table 1 Product parameters of Example 1

[0134]

[0135]

[0136] As can be seen from Table 1, the high-iron red mud and refractory limonite selected from a certain place in Henan Province were treated by the method provided in the embodiments of the present application to obtain an iron concentrate with a yield of 63.83%, a total iron content of 60.42%, and a low impurity content (Na2O+K2O content of 0.15%, Al2O3 content of 1.95% and TiO2 content of 0.32%), as well as tailings with a total iron content of 17.97%; the obtained iron concentrate can be used as a raw material for steel smelting, and the obtained tailings can be used as a raw material for cement production and a direct sales raw material for concrete, thereby realizing the full quantitative utilization of high-iron red mud and refractory iron ore.

[0137] Example 2

[0138] High-iron red mud and refractory limonite from a certain place in Guangxi Zhuang Autonomous Region were selected. The chemical composition of the high-iron red mud met the following requirements by mass fraction: Al2O3: 8.56%, SiO2: 16.52%, TFe: 45.82%. In addition, the iron-containing minerals in the high-iron red mud are mainly aluminous goethite and red mud ore, wherein the mass ratio of aluminous goethite to iron-containing minerals is 0.4122. There are other gangue minerals in the high-iron red mud, including gibbsite, cancrystal, gibbsite and a small amount of diaspore.

[0139] Refractory iron ore is refractory limonite. In terms of mass fraction, the main chemical components of refractory limonite meet the following requirements: TFe: 39.72%, Al2O3: 1.28%, SiO2: 16.42%. In addition, limonite is the main iron-bearing mineral in refractory limonite, with a small amount of hematite, and the rest are gangue minerals, which are mainly quartz, dolomite, etc.

[0140] like Figure 2 As shown, a method for synergistic utilization of red mud and refractory iron ore comprises the steps of:

[0141] S1. Using an ultra-high pressure filter press to dehydrate the red mud mainly by filter pressing dehydration to obtain dehydrated red mud and filtrate; wherein the filtrate can be comprehensively recycled;

[0142] S2. drying and breaking up the dehydrated red mud using the roasting tail gas of the suspended magnetized roasting furnace to obtain dry red mud and drying tail gas, respectively;

[0143] S3. crushing, dry grinding and dry magnetic separation of the refractory iron ore to obtain a rough iron concentrate and a first tailings;

[0144] S4. The crude iron concentrate and the dry red mud are mixed, and then granulated using a granulator to obtain roasted raw material particles;

[0145] S5. Drying the roasted raw meal particles using drying exhaust gas to obtain dry raw meal;

[0146] S6. The dry raw material is subjected to suspended magnetization roasting in a reducing atmosphere, and then rapidly cooled by water quenching to obtain magnetized roasted clinker;

[0147] S7. Wet grinding the magnetized roasted clinker, and then performing weak magnetic separation to obtain iron concentrate and second tailings, respectively;

[0148] S8. merging the first tailings and the second tailings to obtain tailings;

[0149] The mass ratio of dry red mud to rough iron concentrate is 40:60.

[0150] The moisture content of dehydrated red mud is 19.21%;

[0151] The moisture content of dry red mud is 12.52%;

[0152] The moisture content of the dry raw meal was 4.95%.

[0153] The diameter of the roasted raw material particles is 0.8 mm.

[0154] The reducing atmosphere includes a carbon monoxide atmosphere, and the carbon monoxide volume concentration of the carbon monoxide atmosphere is 3.80%;

[0155] The temperature of suspended magnetization calcination is 650°C, and the time of suspended magnetization calcination is 2.0 min.

[0156] The terminal grinding fineness of wet grinding satisfies: the mass ratio of the first fine-grained material to the magnetized roasted clinker is 69.85%; wherein the particle size of the first fine-grained material is ≤0.038 mm.

[0157] The weak magnetic separation process includes weak magnetic roughing and weak magnetic concentrating. The magnetic field strength of the weak magnetic roughing is 0.40T, and the magnetic field strength of the weak magnetic concentrating is 0.30T.

[0158] The pretreatment includes crushing, dry grinding and dry magnetic separation. The terminal grinding fineness of dry grinding satisfies: the mass ratio of the second fine particle size material to the refractory iron ore is 74.85%; the particle size of the second fine particle size material is ≤0.038mm.

[0159] Dry magnetic separation treatment includes dry roughing and dry scavenging. The magnetic field intensity of dry roughing is 0.6T, and the magnetic field intensity of dry scavenging is 1.1T.

[0160] The product parameters of the iron ore concentrate, the first tailings, the iron ore concentrate, the second tailings and the roasted raw material particles obtained in each step are shown in Table 2.

[0161] Table 2 Product parameters of Example 2

[0162]

[0163] It can be seen from Table 2 that the high-iron red mud and refractory limonite selected from a certain place in Guangxi Zhuang Autonomous Region were treated by the method provided in the embodiments of the present application to obtain an iron concentrate with a yield of 70.12%, a total iron content of 61.68%, and a low impurity content (Na2O+K2O content of 0.18%, Al2O3 content of 1.52% and TiO2 content of 0.32%), as well as tailings with a total iron content of 21.24%; the obtained iron concentrate can be used as a raw material for steel smelting, and the obtained tailings can be used as a raw material for cement production and a direct sales raw material for concrete, thereby realizing the full quantitative utilization of high-iron red mud and refractory iron ore.

[0164] Example 3

[0165] High-iron red mud and refractory siderite from a certain place in Shandong were selected. The chemical composition of the high-iron red mud met the following requirements by mass fraction: Al2O3: 12.32%, SiO2: 5.79%, TFe: 38.56%. In addition, the iron-containing minerals in the high-iron red mud are mainly aluminous goethite and red mud ore, wherein the mass ratio of aluminous goethite to iron-containing minerals is 0.5478. There are other gangue minerals in the high-iron red mud, including boehmite, gibbsite, gibbsite and a small amount of diaspore.

[0166] Refractory iron ore is refractory siderite. In terms of mass fraction, the main chemical components of refractory siderite meet the following requirements: TFe: 29.31%, Al2O3: 2.21%, SiO2: 19.47%. In addition, siderite and limonite are the main iron-bearing minerals in refractory siderite. The mass ratio of siderite to refractory siderite is 0.8125, and the mass ratio of limonite to refractory siderite is 0.1041. The rest are gangue minerals, which are mainly quartz and sericite, followed by chlorite, and a small amount of feldspar, dolomite, barite, etc.

[0167] like Figure 2 As shown, a method for synergistic utilization of red mud and refractory iron ore comprises the steps of:

[0168] S1. Using an ultra-high pressure filter press to dehydrate the red mud mainly by filter pressing dehydration to obtain dehydrated red mud and filtrate; wherein the filtrate can be comprehensively recycled;

[0169] S2. drying and breaking up the dehydrated red mud using the roasting tail gas of the suspended magnetized roasting furnace to obtain dry red mud, the first tailings and the drying tail gas, respectively;

[0170] S3. crushing, dry grinding and dry magnetic separation of refractory iron ore to obtain rough iron concentrate;

[0171] S4. The crude iron concentrate and the dry red mud are mixed, and then granulated using a granulator to obtain roasted raw material particles;

[0172] S5. Drying the roasted raw meal particles using drying exhaust gas to obtain dry raw meal;

[0173] S6. The dry raw material is subjected to suspended magnetization roasting in a reducing atmosphere, and then rapidly cooled by water quenching to obtain magnetized roasted clinker;

[0174] S7. Wet grinding the magnetized roasted clinker, and then performing weak magnetic separation to obtain iron concentrate and second tailings, respectively;

[0175] S8. merging the first tailings and the second tailings to obtain tailings;

[0176] The mass ratio of dry red mud to rough iron concentrate is 30:70.

[0177] The moisture content of dehydrated red mud is 20.52%;

[0178] The moisture content of dry red mud is 12.85%;

[0179] The moisture content of the dry raw meal is 4.78%.

[0180] The diameter of the roasted raw material particles is 2.0 mm.

[0181] The reducing atmosphere includes a carbon monoxide atmosphere, and the carbon monoxide volume concentration of the carbon monoxide atmosphere is 4.50%;

[0182] The temperature of suspended magnetization roasting is 850°C, and the time of suspended magnetization roasting is 3.5 min.

[0183] The terminal grinding fineness of wet grinding satisfies: the mass ratio of the first fine-grained material to the magnetized roasted clinker is 69.25%; wherein the particle size of the first fine-grained material is ≤0.038 mm.

[0184] The weak magnetic separation process includes weak magnetic roughing and weak magnetic concentrating. The magnetic field strength of the weak magnetic roughing is 0.40T, and the magnetic field strength of the weak magnetic concentrating is 0.30T.

[0185] The pretreatment includes crushing, dry grinding and dry magnetic separation. The terminal grinding fineness of dry grinding satisfies that the mass ratio of the second fine particle size material to the refractory iron ore is 75.23%. The particle size of the second fine particle size material is ≤0.038 mm.

[0186] Dry magnetic separation treatment includes dry roughing and dry scavenging. The magnetic field strength of dry roughing is 0.8T, and the magnetic field strength of dry scavenging is 1.3T.

[0187] The product parameters of the iron ore concentrate, the first tailings, the iron ore concentrate, the second tailings and the roasted raw material particles obtained in each step are shown in Table 3.

[0188] Table 3 Product parameters of Example 3

[0189]

[0190] It can be seen from Table 3 that high-iron red mud and refractory siderite from a certain place in Shandong were selected and treated by the method provided in the embodiments of the present application to obtain an iron concentrate with a yield of 54.08%, a total iron content of 61.37%, and a low impurity content (Na2O+K2O content of 0.19%, Al2O3 content of 1.79% and TiO2 content of 0.31%), as well as tailings with a total iron content of 14.20%; the obtained iron concentrate can be used as a raw material for steel smelting, and the obtained tailings can be used as a raw material for cement production and a direct sales raw material for concrete, thereby realizing the full quantitative utilization of high-iron red mud and refractory iron ore.

[0191] Example 4

[0192] High-iron red mud and refractory siderite from a certain place in Yunnan were selected. The chemical composition of the high-iron red mud met the following requirements: Al2O3: 8.52%, SiO2: 9.79%, TFe: 35.71% by mass fraction. In addition, the iron-containing minerals in the high-iron red mud are mainly aluminous goethite and red mud ore, wherein the mass ratio of aluminous goethite to iron-containing minerals is 0.6171. The high-iron red mud also contains other gangue minerals, including hydrated garnet, perovskite, gibbsite, diaspore and a small amount of boehmite.

[0193] The refractory iron ore is refractory siderite. In terms of mass fraction, the main chemical components of refractory siderite meet the following requirements: TFe: 30.94%, Al2O3: 1.52%, SiO2: 15.33%. In addition, the refractory siderite is mainly an iron-bearing mineral, with a small amount of limonite. The mass ratio of siderite to refractory siderite is 0.8677, and the mass ratio of limonite to refractory siderite is 0.0908. The rest are gangue minerals, which are mainly quartz and muscovite, followed by calcite and a small amount of chlorite.

[0194] like Figure 2 As shown, a method for synergistic utilization of red mud and refractory iron ore comprises the steps of:

[0195] S1. Using an ultra-high pressure filter press to dehydrate the red mud mainly by filter pressing dehydration to obtain dehydrated red mud and filtrate; wherein the filtrate can be comprehensively recycled;

[0196] S2. drying and breaking up the dehydrated red mud using the roasting tail gas of the suspended magnetized roasting furnace to obtain dry red mud, the first tailings and the drying tail gas, respectively;

[0197] S3. crushing, dry grinding and dry magnetic separation of refractory iron ore to obtain rough iron concentrate;

[0198] S4. The crude iron concentrate and the dry red mud are mixed, and then granulated using a granulator to obtain roasted raw material particles;

[0199] S5. Drying the roasted raw meal particles using drying exhaust gas to obtain dry raw meal;

[0200] S6. The dry raw material is subjected to suspended magnetization roasting in a reducing atmosphere, and then rapidly cooled by water quenching to obtain magnetized roasted clinker;

[0201] S7. Wet grinding the magnetized roasted clinker, and then performing weak magnetic separation to obtain iron concentrate and second tailings, respectively;

[0202] S8. merging the first tailings and the second tailings to obtain tailings;

[0203] The mass ratio of dry red mud to rough iron concentrate is 60:40.

[0204] The moisture content of dehydrated red mud is 19.33%;

[0205] The moisture content of dry red mud is 13.33%;

[0206] The moisture content of the dry raw meal was 4.09%.

[0207] The diameter of the roasted raw material particles is 2.2 mm.

[0208] The reducing atmosphere includes a carbon monoxide atmosphere, and the carbon monoxide volume concentration of the carbon monoxide atmosphere is 5.50%;

[0209] The temperature of suspended magnetization roasting is 900°C, and the time of suspended magnetization roasting is 3.0 min.

[0210] The terminal grinding fineness of wet grinding satisfies: the mass ratio of the first fine-grained material to the magnetized roasted clinker is 73.52%; wherein the particle size of the first fine-grained material is ≤0.038 mm.

[0211] The weak magnetic separation process includes weak magnetic roughing and weak magnetic concentrating. The magnetic field strength of the weak magnetic roughing is 0.30T, and the magnetic field strength of the weak magnetic concentrating is 0.20T.

[0212] The pretreatment includes crushing, dry grinding and dry magnetic separation. The terminal grinding fineness of dry grinding satisfies that the mass ratio of the second fine particle size material to the refractory iron ore is 80.23%. The particle size of the second fine particle size material is ≤0.038mm.

[0213] Dry magnetic separation treatment includes dry roughing and dry scavenging. The magnetic field strength of dry roughing is 0.8T, and the magnetic field strength of dry scavenging is 1.3T.

[0214] The product parameters of the rough iron concentrate, the first tailings, the iron concentrate, the second tailings and the roasted raw material particles obtained in each step are shown in Table 4.

[0215] Table 4 Product parameter table of Example 4

[0216]

[0217] It can be seen from Table 4 that by selecting high-iron red mud and refractory siderite from a certain place in Yunnan Province and treating them with the method provided in the embodiments of the present application, an iron concentrate with a yield of 50.96%, a total iron content of 60.39%, and a low impurity content (Na2O+K2O content of 0.19%, Al2O3 content of 1.79% and TiO2 content of 0.29%), as well as tailings with a total iron content of 16.22% can be obtained; the obtained iron concentrate can be used as a raw material for steel smelting, and the obtained tailings can be used as a raw material for cement production and a direct sales raw material for concrete, thereby realizing the full quantitative utilization of high-iron red mud and refractory iron ore.

[0218] Example 5

[0219] High-iron red mud and refractory oolitic hematite from a certain place in Shanxi Province were selected. The chemical composition of the high-iron red mud met the following requirements: Al2O3: 12.47%, SiO2: 6.21%, TFe: 36.49% by mass fraction. In addition, the iron-containing minerals in the high-iron red mud are mainly aluminous goethite and red mud ore, wherein the mass ratio of aluminous goethite to iron-containing minerals is 0.5739. There are other gangue minerals in the high-iron red mud, including sodium silicate slag, hydrated garnet, gibbsite, diaspore, perovskite, rutile and a small amount of diaspore.

[0220] Refractory iron ore is refractory oolitic hematite. In terms of mass fraction, the main chemical components of refractory oolitic hematite meet the following requirements: TFe: 39.52%, Al2O3: 4.33%, SiO2: 16.42%. In addition, the vein mineral in refractory oolitic hematite is quartz, followed by kaolinite and mica. Refractory oolitic hematite also includes other silicate minerals such as montmorillonite and illite in small amounts.

[0221] like Figure 2 As shown, a method for synergistic utilization of red mud and refractory iron ore comprises the steps of:

[0222] S1. Using an ultra-high pressure filter press to dehydrate the red mud mainly by filter pressing dehydration to obtain dehydrated red mud and filtrate; wherein the filtrate can be comprehensively recycled;

[0223] S2. drying and breaking up the dehydrated red mud using the roasting tail gas of the suspended magnetized roasting furnace to obtain dry red mud, the first tailings and the drying tail gas, respectively;

[0224] S3. crushing, dry grinding and dry magnetic separation of refractory iron ore to obtain rough iron concentrate;

[0225] S4. The crude iron concentrate and the dry red mud are mixed, and then granulated using a granulator to obtain roasted raw material particles;

[0226] S5. Drying the roasted raw meal particles using drying exhaust gas to obtain dry raw meal;

[0227] S6. The dry raw material is subjected to suspended magnetization roasting in a reducing atmosphere, and then rapidly cooled by water quenching to obtain magnetized roasted clinker;

[0228] S7. Wet grinding the magnetized roasted clinker, and then performing weak magnetic separation to obtain iron concentrate and second tailings, respectively;

[0229] S8. merging the first tailings and the second tailings to obtain tailings;

[0230] The mass ratio of dry red mud to rough iron concentrate is 30:70.

[0231] The moisture content of dehydrated red mud is 20.45%;

[0232] The moisture content of dry red mud is 12.85%;

[0233] The moisture content of the dry raw meal is 6.22%.

[0234] The diameter of the roasted raw material particles is 1.8 mm.

[0235] The reducing atmosphere includes a carbon monoxide atmosphere, and the carbon monoxide volume concentration of the carbon monoxide atmosphere is 5.00%;

[0236] The temperature of suspended magnetization roasting is 800°C, and the time of suspended magnetization roasting is 2.8 min.

[0237] The terminal grinding fineness of wet grinding satisfies: the mass ratio of the first fine-grained material to the magnetized roasted clinker is 75.58%; wherein the particle size of the first fine-grained material is ≤0.038 mm.

[0238] The weak magnetic separation process includes weak magnetic roughing and weak magnetic concentrating. The magnetic field strength of the weak magnetic roughing is 0.45T, and the magnetic field strength of the weak magnetic concentrating is 0.30T.

[0239] The pretreatment includes crushing, dry grinding and dry magnetic separation. The terminal grinding fineness of dry grinding satisfies: the mass ratio of the second fine particle size material to the refractory iron ore is 70.33%; the particle size of the second fine particle size material is ≤0.038mm.

[0240] Dry magnetic separation treatment includes dry roughing and dry scavenging. The magnetic field intensity of dry roughing is 0.8T, and the magnetic field intensity of dry scavenging is 1.2T.

[0241] The product parameters of the iron ore concentrate, the first tailings, the iron ore concentrate, the second tailings and the roasted raw material particles obtained in each step are shown in Table 5.

[0242] Table 5 Product parameters of Example 5

[0243]

[0244] It can be seen from Table 5 that high-iron red mud and refractory oolitic hematite from a certain place in Shanxi were selected and treated by the method provided in the embodiments of the present application to obtain an iron concentrate with a yield of 60.33%, a total iron content of 62.75%, and a low impurity content (Na2O+K2O content of 0.18%, Al2O3 content of 1.58% and TiO2 content of 0.26%), as well as tailings with a total iron content of 18.83%; the obtained iron concentrate can be used as a raw material for steel smelting, and the obtained tailings can be used as a raw material for cement production and a direct sales raw material for concrete, thereby realizing the full quantitative utilization of high-iron red mud and refractory iron ore.

[0245] Comparative Example 1

[0246] Based on the high-iron red mud raw material selected in Example 1, the total iron content of the high-iron red mud is 38.35% by mass fraction; the iron-containing minerals in the high-iron red mud are mainly alnicotinite and hematite, wherein the mass ratio of alnicotinite to iron-containing minerals is 0.5675. Then, the prior art (1) in the background technology is used for treatment, and the component contents of the obtained products are shown in Table 6.

[0247] Table 6 Component content distribution of each product of Comparative Example 1

[0248]

[0249] Comparative Example 2

[0250] Based on the high-iron red mud raw material selected in Example 2, the total iron content of the high-iron red mud is 45.82% by mass fraction; the iron-containing minerals in the high-iron red mud are mainly alnicotinite and hematite, wherein the mass ratio of alnicotinite to iron-containing minerals is 0.4122. Then, the prior art (1) in the background technology is used for treatment, and the component contents of the obtained products are shown in Table 7.

[0251] Table 7 Component content distribution of each product of Comparative Example 2

[0252]

[0253] Comparative Example 3

[0254] Based on the high-iron red mud raw material selected in Example 3, the total iron content of the high-iron red mud is 38.56% by mass fraction; the iron-containing minerals in the high-iron red mud are mainly alnicotinite and hematite, wherein the mass ratio of alnicotinite to iron-containing minerals is 0.5478. Then, the prior art (1) in the background technology is used for treatment, and the component contents of the obtained products are shown in Table 8.

[0255] Table 8 Component content distribution of each product of Comparative Example 3

[0256]

[0257] Comparative Example 4

[0258] Based on the high-iron red mud raw material selected in Example 4, the total iron content of the high-iron red mud is 35.71% by mass fraction; the iron-containing minerals in the high-iron red mud are mainly alnicotinite and hematite, wherein the mass ratio of alnicotinite to iron-containing minerals is 0.6171. Then, the prior art (1) in the background technology is used for treatment, and the component contents of the obtained products are shown in Table 8.

[0259] Table 9 Component content distribution of each product of Comparative Example 4

[0260]

[0261] Comparative Example 5

[0262] Based on the high-iron red mud raw material selected in Example 5, the total iron content of the high-iron red mud is 35.71% by mass fraction; the iron-containing minerals in the high-iron red mud are mainly alnicotinite and hematite, wherein the mass ratio of alnicotinite to iron-containing minerals is 0.5739. Then, the prior art (1) in the background technology is used for treatment, and the component contents of the obtained products are shown in Table 8.

[0263] Table 10 Component content distribution of each product of Comparative Example 5

[0264]

[0265] Comparative Example 6

[0266] The high iron raw material and refractory limonite disclosed in Example 1 are further modified as follows:

[0267] The mass ratio of dry red mud to rough iron concentrate is 1:9. The results are shown in Table 11.

[0268] Table 11 Component content distribution of each product of Comparative Example 6

[0269]

[0270] Comparative Example 7

[0271] The high iron raw material and refractory limonite disclosed in Example 1 are further modified as follows:

[0272] The mass ratio of dry red mud to rough iron concentrate is 9:1. The results are shown in Table 12.

[0273] Table 12 Component content distribution of each product of Comparative Example 7

[0274]

[0275]

[0276] Comparative Example 8

[0277] The high iron raw material and refractory limonite disclosed in Example 1 are further modified as follows:

[0278] The carbon monoxide volume concentration of the carbon monoxide atmosphere is 2.0%. The results are shown in Table 13.

[0279] Table 13 Component content distribution of each product of Comparative Example 8

[0280]

[0281] Comparative Example 9

[0282] The high iron raw material and refractory limonite disclosed in Example 1 are further modified as follows:

[0283] The carbon monoxide volume concentration of the carbon monoxide atmosphere is 6.0%. The results are shown in Table 14.

[0284] Table 14 Component content distribution of each product of Comparative Example 9

[0285]

[0286]

[0287] Related experiments and effect data:

[0288] The products obtained by the methods of each embodiment and each comparative example were statistically analyzed, and the results are shown in Table 15.

[0289] Table 15 Statistics of various products of the embodiments and comparative examples

[0290]

[0291]

[0292] It can be seen from Table 15 that the method for the coordinated utilization of red mud and refractory iron ore provided in the embodiment of the present application, the obtained iron concentrate has a total iron content of ≥60.39%. The impurity content (Al2O3, K2O+Na2O, TiO2) in the iron concentrate is low, which can meet the C60 requirement in the national quality standard for iron concentrate GB / T36704-2018; in addition, the total iron recovery rate of this method is high; while Comparative Examples 1 to Comparative Examples 5 use the method of the prior art for the same high-iron red mud, the total iron content in the obtained iron concentrate is 56.02% to 58.31%, which is much lower than the total iron content in the iron concentrate obtained in each embodiment, while the impurity content (Al2O3, K2O+Na2O, TiO2) is much higher than the iron concentrate obtained in each embodiment; at the same time, the burn loss (loss on ignition) of Comparative Examples 1 to Comparative Examples 5 + scarring) is much higher than that of each embodiment. This is because the high-iron red mud will experience equipment scarring and fine particle loss during the suspended magnetization roasting process using the method provided in the comparative example, which will lead to loss of iron-containing minerals, and will also affect the service life of the equipment and the quality of the iron concentrate. Problems; Comparative Examples 6 to Comparative Examples 9 are obtained by changing the ratio of dry red mud to iron coarse concentrate and the concentration of carbon monoxide in the reducing gas in Example 1. It is found that the sorting indicators (yield and TFe content) of the iron concentrate obtained by Comparative Examples 6 to Comparative Examples 9 are not as good as those in Example 1, indicating that the conditions of the embodiments are optimal; in addition, each embodiment can also combine the first tailings and the second tailings to obtain tailings, which can be modified by the method provided in the embodiments of the present application to meet the preparation requirements of cement and concrete, or these tailings can be sold as raw materials for preparing silicate cement and concrete.

[0293] In summary, the embodiment of the present application provides a method for the coordinated utilization of red mud and difficult-to-select iron ore. Through the dehydration treatment of high-efficiency filter press, the drying of roasting tail gas and drying tail gas by suspended magnetic roasting, and the staged dehydration and drying technology of dry material mixing, it can effectively reduce the moisture content of red mud and the energy consumption required for drying, solve the problems of high moisture content of red mud and high energy consumption of direct drying, and also save drying costs and improve the application prospects of the overall technology.

[0294] In addition, an embodiment of the present application provides a method for the coordinated utilization of red mud and refractory iron ore. By mixing and granulating the red mud and the iron ore concentrate obtained by pre-treatment of the refractory iron ore, and then combining it with the suspended magnetized roasting technology, the particle size of the roasted raw material particles can be increased, thereby improving the fluidity of the material, thereby solving technical problems such as easy scarring of red mud and refractory iron ore and easy damage to fine particles during the suspended roasting process; in addition, the suspended magnetized roasting technology is used to directionally convert the weakly magnetic iron-containing minerals in the red mud of the dry raw material and the iron ore concentrate into strongly magnetic magnetite, thereby solving the problem that conventional magnetic separation technology cannot obtain qualified iron concentrate and high-iron red mud.

[0295] In addition, an embodiment of the present application provides a method for the coordinated utilization of red mud and refractory iron ore, which uses the iron coarse concentrate obtained by dry magnetic separation of the refractory iron ore and red mud for granulation. The water content, iron mineral content and impurity content of the red mud can be regulated by using the similar characteristics of the coarse concentrate and the iron-containing minerals in the high-iron red mud, so that the elemental composition and phase composition of the roasted raw material particles can be adjusted. This solves the technical problems of high energy consumption in red mud drying, "scarring" of suspended magnetic roasting, high impurity content of iron concentrate and serious loss of fine particles, and realizes the efficient recycling of iron-containing minerals in high-iron red mud and refractory iron ore.

[0296] In addition, the method for the coordinated utilization of red mud and refractory iron ore provided in the embodiment of the present application can not only improve the utilization rate of red mud in alumina enterprises, but also provide high-quality raw materials for the steel industry to reduce the dependence on steel raw materials; in addition, the tailings can also be sold as raw materials for the preparation of cement and concrete, realizing the coordinated and full-scale utilization of high-iron red mud and refractory iron ore, which has the advantages of low cost, high economic benefit, good quality of iron ore concentrate, high resource utilization, mature and stable process, and environmental friendliness.

[0297] The above is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. It will be apparent to those skilled in the art that various modifications to these embodiments are possible, and the general principles defined in the present application can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to these embodiments shown in the present application, but will conform to the widest scope consistent with the principles and novel features applied for by the present application.

Claims

1. A method for the coordinated utilization of red mud and refractory iron ore, characterized in that: The method comprises: Dehydrating the red mud to obtain dehydrated red mud; Drying and breaking up the dehydrated red mud to obtain dry red mud; Pre-treating refractory iron ore to obtain rough iron concentrate; The crude iron concentrate and the dry red mud are mixed, and then granulated to obtain roasted raw material particles; Drying the roasted raw meal particles to obtain dry raw meal; The dry raw material is subjected to suspended magnetization roasting in a reducing atmosphere, and then water quenching to obtain magnetization roasted clinker; Wet grinding the magnetized roasted clinker and then performing weak magnetic separation to obtain iron concentrate; Wherein, the weight ratio of the particulate material with a particle size of less than 0.023 mm in the red mud to the red mud is 0.4 to 0.8; The diameter of the roasted raw material particles is 0.5 mm to 2.5 mm; The mass ratio of the dry red mud to the rough iron concentrate is 2:8 to 6:

4.

2. The method according to claim 1, characterized in that The ratio of the total iron content of the red mud to the total weight of the red mud is ≥0.3; The ratio of the total iron content of the refractory iron ore to the total weight of the refractory iron ore is ≥0.25, and the refractory iron ore includes at least one of the following: Refractory limonite, refractory siderite and refractory oolitic hematite.

3. The method according to claim 1, characterized in that The moisture content of the dehydrated red mud is ≤21%; The moisture content of the dry red mud is 7% to 14%; The moisture content of the dry raw material is 4% to 7.5%.

4. The method according to claim 1, characterized in that: The drying medium used in the drying is the roasting tail gas of the suspended magnetization roasting; The drying medium used in the drying is the drying tail gas from the drying.

5. The method according to claim 1, characterized in that The reducing atmosphere comprises a carbon monoxide atmosphere, wherein the carbon monoxide volume concentration of the carbon monoxide atmosphere is 3.5% to 5.5%; The temperature of the suspended magnetization roasting is 500° C. to 900° C., and the time of the suspended magnetization roasting is 0.5 min to 3.5 min.

6. The method according to claim 1, characterized in that The terminal grinding fineness of the wet grinding satisfies: the mass ratio of the first fine-grained material to the magnetized roasted clinker is 60% to 75%; wherein the particle size of the first fine-grained material is ≤0.038 mm.

7. The method according to claim 1, characterized in that The weak magnetic separation process includes weak magnetic roughing and weak magnetic concentrating. The magnetic field strength of the weak magnetic roughing is 0.3T to 0.5T, and the magnetic field strength of the weak magnetic concentrating is 0.1T to 0.3T.

8. The method according to claim 1, characterized in that The pretreatment includes crushing, dry grinding and dry magnetic separation; wherein the terminal grinding fineness of the dry grinding satisfies: the mass ratio of the second fine-grained material to the difficult-to-select iron ore is 60% to 85%; wherein the particle size of the second fine-grained material is ≤0.038mm.

9. The method according to claim 8, characterized in that The dry magnetic separation process includes dry roughing and dry sweeping. The magnetic field strength of the dry roughing is 0.5T to 0.9T, and the magnetic field strength of the dry sweeping is 1.0T to 1.3T.

10. The method according to claim 1, characterized in that The total iron content of the iron concentrate is ≥60%, the total content of sodium oxide and potassium oxide of the iron concentrate is ≤0.20%, the aluminum oxide content of the iron concentrate is ≤2.0%, and the titanium oxide content of the iron concentrate is ≤0.35%.

Citation Information

Cited By

  • Method for synergistically utilizing red mud and refractory iron ore

    WO2026040441A1