Ultrafine grain oxygen-free copper bar and preparation method thereof

The preparation of ultrafine crystal oxygen-free copper rods through multi-stage processes has solved the problem of insufficient strength of pure copper rods, and achieved the improvement of mechanical properties and electrical conductivity of high-quality oxygen-free copper rods, meeting the high-performance needs of electronic products.

CN119040652APending Publication Date: 2024-11-29YANTAI WANLONG VACUUM METALLURGY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411156124.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing pure copper rods are insufficient in strength and cannot meet the needs of miniaturization and integration of electronic products. It is necessary to develop high-quality ultrafine crystal oxygen-free copper rods to improve mechanical properties.

Method used

Through multi-stage processes such as vacuum casting, preheating treatment, hot forging deformation, hot extrusion deformation, drawing and recrystallization annealing, the grain size is controlled below 25μm to ensure the ultrafine crystal structure and high purity of the oxygen-free copper rod. .

Benefits of technology

The ultrafine crystal oxygen-free copper rod is prepared, with excellent mechanical properties and high conductivity, meeting the market demand of high-performance electronic materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040652A_ABST
    Figure CN119040652A_ABST
Patent Text Reader

Abstract

The invention discloses an ultra-fine grain oxygen-free copper bar and a preparation method thereof. The preparation method comprises the following specific steps: vacuum casting: putting electrolytic copper into a vacuum melting furnace, heating to 1100-1200 DEG C until furnace charge is completely melted down, vacuumizing for 10-30 minutes, filling nitrogen to break vacuum, and casting and forming; an oxygen-free copper cast ingot obtained through vacuum casting is put into a heat preservation furnace to be preheated, the preheating temperature ranges from 800 DEG C to 900 DEG C, and the heat preservation time ranges from 2 hours to 3 hours; hot forging deformation is conducted, specifically, the preheated oxygen-free copper cast ingot is subjected to hot forging, the deformation amount of primary hot forging is 60%-70%, secondary hot forging is conducted after remelting and heat preservation is conducted, the deformation amount is 60%-70%, third hot forging is conducted after remelting and heat preservation is conducted again, the deformation amount is 50%-60%, and the hot forging temperature is always larger than 750-800 DEG C; the oxygen-free copper cast ingot obtained after hot forging is preheated to 800-900 DEG C, hot extrusion is conducted, and the extrusion deformation is 70%-75%; drawing is conducted, specifically, the extruded oxygen-free copper cast ingot is drawn, and the drawing deformation is 60-70%; and recrystallization annealing is conducted, specifically, the drawn oxygen-free copper cast ingot is annealed for 1-2 hours at the temperature of 400-420 DEG C, air cooling is conducted after annealing, and the oxygen-free copper bar with the average grain size smaller than 25 micrometers is obtained. According to the technical scheme, preparation of the oxygen-free copper bar is achieved through a series of accurately-controlled process steps.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of copper alloy preparation, and in particular relates to an ultrafine-grained oxygen-free copper rod and a preparation method thereof. Background Art

[0002] With the rapid development of electronic information technology, the requirements for electronic components are getting higher and higher. As one of the important electronic materials, oxygen-free copper occupies an important position in the electronics industry. Due to its good electrical conductivity, corrosion resistance and fatigue resistance, oxygen-free copper is widely used in various electronic products.

[0003] Nowadays, ordinary pure copper rods are increasingly unable to meet the needs of industrial development due to their low strength. Therefore, how to improve the strength of copper wire has become the focus of attention. Grain size is the main factor affecting the mechanical properties of traditional polycrystalline materials with grain sizes above the micrometer level. As the grain size decreases, a large number of grain boundary structures exist in the microstructure. Since the grain boundary area is inversely proportional to the grain size, the total grain boundary area per unit volume in ultrafine-grained crystal materials is much higher than that of coarse-grained materials. Since the proportion of grain boundaries in ultrafine-grained materials is greatly increased, their performance must be very different from that of traditional coarse-grained materials with the same chemical composition. As the number of grain boundaries increases, the stress caused by dislocation accumulation increases. Therefore, fine-grained metals should have higher strength and hardness.

[0004] Therefore, under the development trend of miniaturization and integration of electronic products, it is necessary to develop a high-quality ultrafine-grained oxygen-free copper rod to meet the material requirements of various precision electronic products. Summary of the invention

[0005] The object of the present invention is to provide an ultrafine-grained oxygen-free copper rod and a preparation method thereof, thereby solving at least part of the above-mentioned technical problems.

[0006] A first aspect of an embodiment of the present invention provides an ultrafine-grained oxygen-free copper rod and a method for preparing the same, comprising the following steps:

[0007] Vacuum melting and casting: put the electrolytic copper into a vacuum melting furnace, heat it to 1100-1200℃ until the charge is completely melted, evacuate for 10-30 minutes, fill it with nitrogen to break the vacuum, and cast it into shape;

[0008] Preheating treatment: put the oxygen-free copper ingot obtained by vacuum casting into a holding furnace for preheating at a temperature of 800-900°C for 2-3 hours;

[0009] Hot forging deformation: The preheated oxygen-free copper ingot is hot forged, the deformation of the first hot forging is 60%-70%, and the second hot forging is carried out after returning to the furnace for heat preservation, the deformation is 60%-70%, and the third hot forging is carried out after returning to the furnace for heat preservation, the deformation is 50%-60%, and the hot forging temperature is always greater than 750-800℃;

[0010] Hot extrusion deformation: preheat the hot forged oxygen-free copper ingot to 800-900°C and perform hot extrusion, with the extrusion deformation amount being 70%-75%;

[0011] Drawing: The extruded oxygen-free copper ingot is drawn, and the drawing deformation is 60-70%;

[0012] Recrystallization annealing: The drawn oxygen-free copper ingot is annealed at 400-420°C for 1-2 hours, and then air-cooled to obtain an oxygen-free copper rod with an average grain size of less than 25 μm.

[0013] The technical effects achieved are as follows: the present invention performs smelting at a high temperature of 1100-1200°C, ensuring complete melting and uniform mixing of electrolytic copper; 10-30 minutes of vacuum treatment, achieving a temperature below 10 -2 The vacuum degree of Pa can effectively remove the dissolved gas in the copper, prevent oxidation and inclusions, and lay the foundation for obtaining pure oxygen-free copper ingots; preheating for 2-3 hours in the temperature range of 800-900℃ ensures the uniformity of the internal temperature of the oxygen-free copper ingot, provides consistent starting conditions for subsequent hot forging deformation, helps to reduce uneven deformation and internal stress during forging, and creates favorable conditions for grain refinement; the first hot forging deformation is controlled at 60%-70%, and the subsequent two hot forgings are deformed in the same proportion. Such multi-stage deformation helps to gradually break the coarse grain structure of the original cast state and promote grain refinement; the hot forging temperature is maintained above 750-800℃, which ensures the plasticity of the material and avoids cold work hardening; in the temperature range of 800-900℃ Hot extrusion is carried out inside the material, and the deformation is controlled at 70%-75%. This deformation under high temperature and high pressure further refines the grains and promotes the recrystallization process inside the material, providing conditions for obtaining a uniform and fine grain structure; the drawing deformation is controlled at 60-70%. This process further refines the grains through stretching and enhances the density of the material; stress control during the drawing process helps prevent the material from breaking and maintains the continuity and integrity of the material; annealing treatment is carried out within the temperature range of 400-420℃ for 1-2 hours. The precise control of this temperature range and time helps promote the recrystallization process inside the material, eliminates the internal stress generated during forging and drawing, and prevents excessive growth of grains, thereby ensuring that the final product has an ultra-fine grain size.

[0014] Optionally, the purity of the electrolytic copper is greater than 99.95%.

[0015] The technical effect achieved is: by using electrolytic copper with a purity greater than 99.95% as raw material, the high purity characteristics of oxygen-free copper rods are ensured, which helps to reduce impurities in the material, thereby improving its conductivity and corrosion resistance, and provides a basis for obtaining ultrafine-grained oxygen-free copper rods with excellent electrical properties.

[0016] Optionally, during the vacuum casting process, the vacuum degree of the vacuum pump is less than 10 -2 Pa.

[0017] The technical effect achieved is: vacuum is drawn to less than 10 during vacuum casting. -2 The vacuum degree of Pa can effectively remove dissolved gases in the copper material, prevent oxidation and inclusions, ensure the purity of oxygen-free copper, and provide the necessary conditions for the formation of ultrafine grain structure in subsequent steps.

[0018] Optionally, the surface temperature uniformity of the oxygen-free copper ingot after the preheat treatment is controlled within ±5°C.

[0019] The technical effect achieved is: after preheating treatment, the surface temperature uniformity of the oxygen-free copper ingot is controlled within ±5°C. This precise temperature control helps to ensure uniform deformation of the material during the forging process, avoids local overheating or cooling, and provides favorable conditions for the formation of fine and uniform grains.

[0020] Optionally, during the hot forging deformation process, the heat preservation time of the oxygen-free copper ingot after each hot forging does not exceed 5 minutes.

[0021] The technical effect achieved is: after hot forging deformation, the insulation time of the oxygen-free copper ingot does not exceed 5 minutes. This control helps to reduce the risk of oxidation of the material at high temperatures, while maintaining the thermoplasticity of the material, providing a time window for grain refinement and homogenization.

[0022] Optionally, during the hot extrusion deformation process, the extrusion speed of the oxygen-free copper ingot is controlled at 2-5 mm / s.

[0023] The technical effect achieved is: during the hot extrusion deformation process, the extrusion speed is controlled at 2-5mm / s. The precise control of this speed helps the material to deform evenly under high temperature and high pressure, reduces the uneven flow of the material, and promotes further refinement of the grains.

[0024] Optionally, during the drawing process, the drawing speed of the oxygen-free copper ingot is controlled at 1-3 mm / s.

[0025] The technical effect achieved is: the drawing speed is controlled at 1-3mm / s. This speed control helps the material to deform evenly during the stretching process, reduce stress concentration, avoid excessive grain growth, and maintain the fineness and uniformity of the grains.

[0026] Optionally, the air cooling rate after the recrystallization annealing is controlled at 5-10°C / s.

[0027] The technical effect achieved is: the air cooling rate after recrystallization annealing is controlled at 5-10℃ / s. This precise cooling rate helps the uniform growth of grains inside the material, avoids uneven growth of grains, ensures the stability of ultrafine grain size, and provides a guarantee for obtaining ultrafine-grained oxygen-free copper rods with excellent mechanical properties.

[0028] A second aspect of an embodiment of the present invention provides an ultrafine-grained oxygen-free copper rod, which is made by the above-mentioned preparation method.

[0029] The technical effect achieved is: the ultrafine-grained oxygen-free copper rod prepared by the above method has an ultrafine grain size while maintaining high conductivity and good mechanical properties, meeting the market demand for high-performance electronic materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a schematic diagram of a process of an ultrafine-grained oxygen-free copper rod according to an embodiment of the present invention;

[0031] Figure 2 This is a metallographic structure picture of an oxygen-free copper rod after hot forging in an embodiment of the present invention;

[0032] Figure 3 This is a metallographic structure picture of an oxygen-free copper rod after annealing in an embodiment of the present invention. DETAILED DESCRIPTION

[0033] Exemplary embodiments will be described in detail herein, examples of which are shown in the accompanying drawings. When the following description refers to the drawings, the same numbers in different drawings represent the same or similar elements unless otherwise indicated. The modes described in the following exemplary embodiments do not represent all modes consistent with the present invention. Instead, they are merely examples of devices consistent with some aspects of the present invention as detailed in the appended claims.

[0034] The terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. Unless otherwise defined, the technical terms or scientific terms used in the present invention should be understood by people with ordinary skills in the field to which the present invention belongs. The words "first", "second" and similar words used in the present specification and claims do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, words such as "one" or "one" do not indicate a quantitative limitation, but indicate that there is at least one. If only "one" is referred to, it will be separately stated. "Multiple" or "several" means two or more. Unless otherwise specified, words such as "front", "rear", "lower" and / or "upper" are only for the convenience of explanation and are not limited to one position or one spatial orientation. Words such as "include" or "comprise" mean that the elements or objects appearing in front of "include" or "comprise" include the elements or objects listed after "include" or "comprise" and their equivalents, and do not exclude other elements or objects. "Connected" or "connected" and similar words are not limited to physical or mechanical connections, and may include electrical connections, whether direct or indirect. The singular forms "a", "said" and "the" used in the present specification and the appended claims are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.

[0035] Embodiment 1:

[0036] The present invention provides a method for preparing an ultrafine-grained oxygen-free copper rod, which successfully prepares an oxygen-free copper rod with an ultrafine grain size through precisely controlled process steps, which not only ensure the microstructure of the material, but also verify its macroscopic physical properties through subsequent tests. Figure 1 As shown, the specific steps are as follows:

[0037] Vacuum casting: At a vacuum degree of 10 -2 Under the condition of 1.3 Pa, electrolytic copper is put into a vacuum melting furnace, heated to 1150℃ and kept at a constant temperature until the charge is completely melted. In this step, the vacuum environment effectively removes gases and impurities, avoids the formation of oxides, ensures the high purity of the alloy melt, and lays the foundation for the subsequent formation of ultrafine grains.

[0038] Pouring: Fill with nitrogen to break the vacuum, and then pour; Breaking the vacuum by filling with nitrogen helps protect the molten copper from oxidation during the pouring process, and secondly, it can also replace the air dissolved in the molten copper, reduce the formation of pores, and improve the density of the cast part; thirdly, it can also stabilize the internal pressure of the pouring system, ensure that the molten metal flows smoothly from the crucible into the mold, and reduce casting defects caused by pressure fluctuations; finally, nitrogen can help push the molten copper to fill the mold, improve the fluidity of the molten copper, and help obtain castings with complex shapes or thin walls.

[0039] Preheating treatment: The oxygen-free copper ingot is preheated in a preheating furnace, the preheating temperature is controlled at 850°C, and the holding time is set to 2.5 hours. The preheating treatment ensures the uniformity of the internal temperature of the ingot and provides consistent starting conditions for the subsequent hot forging deformation.

[0040] Hot forging deformation: The ingot is first hot forged at high temperature, with the first hot forging deformation of 65%, and then returned to the furnace for heat preservation. This process is repeated, with the second and third hot forging deformations of 65% and 55% respectively, and the hot forging temperature is maintained at 780℃. Hot forging deformation not only promotes the crushing and recrystallization of grains, but also refines the grains. Among them, the metallographic structure of the oxygen-free copper rod after hot forging is as follows Figure 2 shown.

[0041] Extrusion and drawing: The oxygen-free copper ingot after hot forging is preheated to 850℃ and hot extruded, and the extrusion deformation is controlled at 72%. Then it is drawn, and the drawing deformation is 65%. The drawing speed is controlled at 2mm / s to ensure that the material is evenly deformed during the stretching process.

[0042] Annealing: The drawn copper rod is annealed at 410°C for 1.5 hours and then air-cooled. Annealing helps release residual stress inside the material and promotes grain growth to a more uniform size.

[0043] Fine grinding and polishing: The annealed oxygen-free copper rods are finely ground and polished to obtain a smooth surface and precise dimensions to ensure the product's appearance quality and dimensional accuracy.

[0044] After the preparation, the ultrafine-grained oxygen-free copper rod was obtained, and the grain size and distribution of the ultrafine-grained oxygen-free copper rod were analyzed by SEM. Figure 3 As shown, the average grain size is 20 μm, and the grains are evenly distributed without obvious aggregation or segregation.

[0045] The following performance tests were performed on the prepared ultrafine-grained oxygen-free copper rod:

[0046] Conductivity test: Conductivity test was conducted using the standard four-point probe method. The test results showed that the conductivity of the ultrafine-grained oxygen-free copper rod was 58.5MS / m (million Siemens per meter), which is higher than the standard conductivity of ordinary oxygen-free copper (55MS / m), showing the positive effect of ultrafine-grained structure on improving conductivity.

[0047] Tensile strength test: According to ISO 6892-2009 standard, tensile test was carried out to determine tensile strength. The test results show that the tensile strength of ultrafine-grained oxygen-free copper rod reaches 390MPa, which is higher than the tensile strength of traditional coarse-grained oxygen-free copper, proving that ultrafine-grained structure can significantly improve the strength of materials.

[0048] Elongation test: The elongation is also measured by tensile test. The elongation of ultrafine-grained oxygen-free copper rod is 30%, which indicates that the material has good plastic deformation ability and can withstand impact and deformation to a certain extent without breaking.

[0049] Embodiment 2:

[0050] The difference between this embodiment and embodiment 1 is that the process parameters are different, and the specific steps are as follows:

[0051] Vacuum melting: The high-purity electrolytic copper is heated to 1160°C in a vacuum melting furnace and subjected to vacuum treatment for 20 minutes to a vacuum degree of less than 10^-3 Pa.

[0052] Pouring: Fill with nitrogen to break the vacuum, then pour;

[0053] Preheating treatment: The preheating temperature is increased to 870°C and the holding time is adjusted to 3 hours.

[0054] Hot forging deformation: The first hot forging deformation was increased to 70%, the second hot forging deformation was 68%, the third hot forging deformation was 58%, and the hot forging temperature was maintained at 785℃.

[0055] Extrusion and drawing: The extrusion deformation is adjusted to 75%, the drawing deformation is maintained at 65%, and the drawing speed is adjusted to 1.8 mm / s.

[0056] Annealing treatment: the annealing temperature was increased to 415°C and the holding time was adjusted to 1.75 hours.

[0057] Fine grinding and polishing: The dimensional tolerance and straightness requirements after fine grinding and polishing are the same as those in Example 1.

[0058] After the preparation, an ultrafine-grained oxygen-free copper rod was obtained. The grain size and distribution of the ultrafine-grained oxygen-free copper rod were analyzed by SEM. The average grain size was 18 μm, and the grains were evenly distributed without obvious aggregation or segregation.

[0059] The prepared ultrafine-grained oxygen-free copper rod has an electrical conductivity of 59.0MS / m, a tensile strength of 405MPa, and an elongation of 32%.

[0060] Embodiment 3:

[0061] The difference between this embodiment and Embodiment 1 and Embodiment 2 is that the process parameters are different, and the specific steps are as follows:

[0062] Vacuum melting: The high-purity electrolytic copper is heated to 1180°C in a vacuum melting furnace and subjected to vacuum treatment for 25 minutes to a vacuum degree of less than 10^-4 Pa.

[0063] Pouring: Fill with nitrogen to break the vacuum, then pour;

[0064] Preheating treatment: The preheating temperature is increased to 890°C and the holding time is adjusted to 2 hours.

[0065] Hot forging deformation: The first hot forging deformation is set to 75%, the second hot forging deformation is 70%, the third hot forging deformation is 60%, and the hot forging temperature is increased to 795℃.

[0066] Extrusion and drawing: The extrusion deformation is adjusted to 70%, the drawing deformation is increased to 70%, and the drawing speed is set to 2.2 mm / s.

[0067] Annealing treatment: the annealing temperature was set at 420°C and the holding time was set at 2 hours.

[0068] Fine grinding and polishing: The dimensional tolerance and straightness requirements after fine grinding and polishing are the same as those in Example 1.

[0069] After the preparation, an ultrafine-grained oxygen-free copper rod was obtained. The grain size and distribution of the ultrafine-grained oxygen-free copper rod were analyzed by SEM. The average grain size was 22 μm. Although it was slightly increased compared with the size of Example 1, the grain size was still not higher than 25 μm, and the grains were evenly distributed without obvious aggregation or segregation.

[0070] The prepared ultrafine-grained oxygen-free copper rod has an electrical conductivity of 58.0MS / m, a tensile strength of 390MPa, and an elongation of 28%.

[0071] In summary, the present invention performs smelting at a high temperature of 1100-1200°C to ensure complete melting and uniform mixing of electrolytic copper; vacuum treatment for 10-30 minutes to achieve a temperature below 10 -2The vacuum degree of Pa can effectively remove the dissolved gas in the copper, prevent oxidation and inclusions, and lay the foundation for obtaining pure oxygen-free copper ingots; preheating for 2-3 hours in the temperature range of 800-900℃ ensures the uniformity of the internal temperature of the oxygen-free copper ingot, provides consistent starting conditions for subsequent hot forging deformation, helps to reduce uneven deformation and internal stress during forging, and creates favorable conditions for grain refinement; the first hot forging deformation is controlled at 60%-70%, and the subsequent two hot forgings are deformed in the same proportion. Such multi-stage deformation helps to gradually break the coarse grain structure of the original cast state and promote grain refinement; the hot forging temperature is maintained above 750-800℃, which ensures the plasticity of the material and avoids cold work hardening; in the temperature range of 800-900℃ Hot extrusion is carried out inside the material, and the deformation is controlled at 70%-75%. This deformation under high temperature and high pressure further refines the grains and promotes the recrystallization process inside the material, providing conditions for obtaining a uniform and fine grain structure; the drawing deformation is controlled at 60-70%. This process further refines the grains through stretching and enhances the density of the material; stress control during the drawing process helps prevent the material from breaking and maintains the continuity and integrity of the material; annealing treatment is carried out within the temperature range of 400-420℃ for 1-2 hours. The precise control of this temperature range and time helps promote the recrystallization process inside the material, eliminates the internal stress generated during forging and drawing, and prevents excessive growth of grains, thereby ensuring that the final product has an ultra-fine grain size.

[0072] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing an ultrafine-grained oxygen-free copper rod, characterized in that , the preparation method comprises the following steps: Vacuum melting and casting: put the electrolytic copper into a vacuum melting furnace, heat it to 1100-1200℃ until the charge is completely melted, evacuate for 10-30 minutes, fill it with nitrogen to break the vacuum, and cast it into shape; Preheating treatment: The oxygen-free copper ingot obtained by vacuum casting is placed in a holding furnace for preheating at a temperature of 800-900°C for 2-3 hours; Hot forging deformation: The preheated oxygen-free copper ingot is hot forged, the deformation of the first hot forging is 60%-70%, and the second hot forging is carried out after returning to the furnace for heat preservation, the deformation is 60%-70%, and the third hot forging is carried out after returning to the furnace for heat preservation, the deformation is 50%-60%, and the hot forging temperature is always greater than 750-800℃; Hot extrusion deformation: preheat the hot forged oxygen-free copper ingot to 800-900°C and perform hot extrusion, with the extrusion deformation amount being 70%-75%; Drawing: The extruded oxygen-free copper ingot is drawn, and the drawing deformation is 60-70%; Recrystallization annealing: The drawn oxygen-free copper ingot is annealed at 400-420°C for 1-2 hours, and then air-cooled to obtain an oxygen-free copper rod with an average grain size of less than 25 μm.

2. The method for preparing an ultrafine-grained oxygen-free copper rod according to claim 1, characterized in that: The purity of the electrolytic copper is greater than 99.95%.

3. The method for preparing an ultrafine-grained oxygen-free copper rod according to claim 1, characterized in that: During the vacuum casting process, the vacuum degree of the vacuum is not higher than 10 -2 Pa.

4. The method for preparing an ultrafine-grained oxygen-free copper rod according to claim 1, characterized in that: The surface temperature uniformity of the oxygen-free copper ingot after the preheat treatment is controlled within ±5°C.

5. The method for preparing an ultrafine-grained oxygen-free copper rod according to claim 1, characterized in that: During the hot forging deformation process, the heat preservation time of the oxygen-free copper ingot after each hot forging does not exceed 5 minutes.

6. The method for preparing an ultrafine-grained oxygen-free copper rod according to claim 1, characterized in that: During the hot extrusion deformation process, the extrusion speed of the oxygen-free copper ingot is controlled at 2-5 mm / s.

7. The method for preparing an ultrafine-grained oxygen-free copper rod according to claim 1, characterized in that: During the drawing process, the drawing speed of the oxygen-free copper ingot is controlled at 1-3 mm / s.

8. The method for preparing an ultrafine-grained oxygen-free copper rod according to claim 1, characterized in that: The air cooling rate after the recrystallization annealing is controlled at 5-10°C / s.

9. An ultrafine-grained oxygen-free copper rod, characterized in that: The ultrafine-grained oxygen-free copper rod is made by the preparation method according to any one of claims 1 to 8.

Citation Information

Cited By

  • Preparation method of high-impact-toughness deformed pure magnesium and product

    CN121538464A