Method for recycling valuable metal in co-roasted product of retired lithium iron phosphate and ternary positive electrode material

By co-calcining the decommissioned lithium iron phosphate with the ternary positive electrode material and using ammonia immersion reaction and electrochemical deposition, the problem of low selectivity for polymetal recovery in lithium-ion battery recycling is solved, and lithium iron phosphate and ternary positive electrode are realized The efficient resource utilization of polymetals in material co-baking products simplifies the process and reduces resource consumption and environmental pressure.

CN119040656AActive Publication Date: 2024-11-29HUIZHOU HENGCHUANG RUINENG ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411167365.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

Prior Art In the process of lithium-ion battery recycling, the recycling selectivity of valuable metals in the co-baked products of lithium iron phosphate and ternary positive electrode materials is low and the process is complicated, resulting in waste of resources and increased environmental pressure, and a lack of efficient recycling methods.

Method used

By mixing and calculating the decommissioned lithium iron phosphate with the ternary positive electrode material at a molar ratio of 1.5:1, the co-calcined product was obtained, and then placed in (NH4)2SO4-NH3·H2O system for ammonia leaching reaction, and selectively leaching lithium and nickel and cobalt elements, and then nickel and cobalt are recovered by electrochemical deposition and evaporation crystallization, and manganese are recovered by water immersion to achieve efficient resource utilization of polymetals.

Benefits of technology

It realizes efficient recycling of lithium, nickel, cobalt and manganese in co-baked products of lithium iron phosphate and ternary positive electrode materials, simplifies the process, reduces resource consumption and environmental pressure, and provides a simple and efficient method for large-scale lithium-ion battery resource utilization. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040656A_ABST
    Figure CN119040656A_ABST
Patent Text Reader

Abstract

The invention relates to a method for recovering valuable metals in a co-roasted product of decommissioned lithium iron phosphate and a ternary positive electrode material, which comprises the following steps: S1, uniformly mixing decommissioned lithium iron phosphate and a ternary positive electrode material according to a molar ratio of 1.5: 1, putting the mixture into a tubular furnace under the protection of nitrogen, and roasting to obtain a co-roasted product; s2, the obtained co-roasting product is placed in a (NH4) 2SO4-NH3.H2O system for an ammonia leaching reaction, and lithium, nickel and cobalt elements are selectively leached out; s3, after ammonia leaching is finished, an ammonia leaching solution containing lithium, nickel and cobalt ions and ammonia leaching residues containing manganese and iron elements are obtained through solid-liquid separation; s5, nickel and cobalt ions in the ammonia leaching solution are subjected to electro-deposition in an electrolytic tank through an electrochemical deposition method and then are recycled in an alloy form, and lithium remaining in electro-deposition residual liquid is subjected to evaporative crystallization to obtain a Li (NH4) (SO4) product; and S6, manganese in the ammonia leaching residues is subjected to water leaching, an iron slag product and a manganese-containing solution are obtained, the obtained manganese-containing solution is subjected to evaporative crystallization, and a (NH4) 2Mn (SO4) 2.6 H2O product is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of recycling of waste lithium-ion batteries, and in particular to a method for recycling valuable metals in a co-baked product of retired lithium iron phosphate and a ternary positive electrode material. Background Art

[0002] The rapid development of the new energy industry has driven the explosive growth of the production and sales of lithium-ion power batteries. Among them, the installation volume of ternary lithium batteries and lithium iron phosphate batteries is the largest, each accounting for about 45% of the total market. In the process of valuable metal recovery, lithium iron phosphate materials usually need to be oxidized to release high-value lithium resources in the lattice; while ternary materials need to add reducing agents to reduce high-valent transition metals (Ni3+, Co3+ and Mn4+), which is more conducive to the recovery of valuable metals. Heat treatment is a pretreatment method commonly used in the recycling process of retired lithium-ion battery materials. Under anaerobic conditions, lithium iron phosphate and ternary electrode materials can serve as redox agents for each other, complementing each other to complete the redox reactions required by the two electrode materials, thereby avoiding the consumption of additional resources. In addition, in the process of lithium battery recycling, it is inevitable that different types of lithium-ion batteries will be mixed and recycled. The co-roasting method can achieve the "take what you need" of the two electrode materials, and the co-roasted products obtained are conducive to the recovery of valuable metals by hydrometallurgical methods.

[0003] In addition, acid dissolution (organic or inorganic acid) is often used to ionize valuable metals in the hydrometallurgical process, which has low selectivity and causes multiple metals to dissolve into the solution, posing a huge challenge to the subsequent separation and extraction of multiple metals. At the same time, in order to recover valuable metals such as lithium, nickel, cobalt, and manganese in the leachate, it is usually necessary to adopt complicated steps such as precipitation, extraction, stripping, membrane separation, and adsorption. The recovery process is long, the equipment investment is large, and the reagent consumption is huge, which increases the recovery cost and environmental pressure. The co-baked product of lithium iron phosphate and ternary positive electrode materials contains a variety of metal substances including lithium phosphate, nickel monoxide, cobalt monoxide, nickel cobalt, manganese monoxide, and ferroferric oxide. At present, there is no relevant method reported on how to recover valuable metals from the co-baked product.

[0004] Therefore, it is urgent to develop a highly selective, targeted and short process method to achieve efficient recovery of valuable metals in the co-calcination products of lithium iron phosphate and ternary positive electrode materials. Summary of the invention

[0005] Based on this, it is necessary to provide a method for recovering valuable metals in the co-roasting products of retired lithium iron phosphate and ternary positive electrode materials in response to the above problem.

[0006] A method for recovering valuable metals in a co-baked product of retired lithium iron phosphate and a ternary positive electrode material comprises the following steps:

[0007] S1: The retired lithium iron phosphate and the ternary cathode material are uniformly mixed at a molar ratio of 1.5:1 and then placed in a tubular furnace under nitrogen protection for 1.5 hours of calcination at a calcination temperature of 600°C to obtain a co-calcined product;

[0008] S2: placing the obtained co-calcined product in a (NH4)2SO4-NH3·H2O system for ammonia leaching reaction, and selectively leaching lithium, nickel and cobalt elements; selective leaching of lithium, nickel and cobalt elements is achieved through the complexation of ammonium ions.

[0009] S3: After the ammonia leaching is completed, the ammonia leaching solution containing lithium, nickel and cobalt ions and the ammonia leaching residue containing manganese and iron elements are obtained by solid-liquid separation;

[0010] S4: introducing an electrolytic cell having a titanium-based ruthenium-iridium oxide coating electrode as an anode and a titanium plate as a cathode into the ammonia immersion solution;

[0011] S5: Electrodepositing nickel ions and cobalt ions in the ammonia immersion solution in an electrolytic cell by an electrochemical deposition method and recovering them in the form of an alloy, and then evaporating and crystallizing the lithium element remaining in the electrodeposition residual solution to obtain a Li(NH4)(SO4) product;

[0012] S6: The manganese in the ammonia leached slag is leached by water to obtain an iron slag product and a manganese-containing solution, and the obtained manganese-containing solution is evaporated and crystallized to obtain a (NH4)2Mn(SO4)2·6H2O product;

[0013] In one of the embodiments, in step S1, the ternary positive electrode material is one or a mixture of NCM111, NCM523, NCM622, and NCM811 materials.

[0014] In one embodiment, in step S2, the (NH4)2SO4 concentration in the (NH4)2SO4-NH3·H2O system is 1-3 mol / L, the NH3·H2O concentration is 2-4 mol / L, the solid-liquid ratio is 5-20 g / L, the leaching temperature of the ammonia leaching reaction is 60-120°C, and the ammonia leaching time is 1-3 h.

[0015] In one embodiment, in step S5, the voltage in the electrochemical deposition method is 4-8V, and the electrolysis is performed at room temperature for 3-9h.

[0016] In one embodiment, in step S6, the solid-liquid ratio in the water immersion method is 50-150 g / L, the temperature is 25-90° C., and the reaction time is 0.5 h.

[0017] The above-mentioned method for recovering valuable metals in the co-roasting products of retired lithium iron phosphate and ternary positive electrode materials is highly targeted and easy to implement. It provides a simple and efficient idea for the recovery of multi-electrode material blends in the process of large-scale lithium-ion battery resource utilization, and realizes the efficient resource utilization of multiple metals in the co-roasting products of retired lithium iron phosphate and ternary positive electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a schematic diagram of the technical process of the present invention;

[0019] Figure 2 is the XRD diagram of the ammonia leached residue in Example 1;

[0020] Figure 3 This is a SEM-EDS image of the nickel-cobalt alloy obtained by electrochemical co-deposition in Example 1;

[0021] Figure 4 This is the XRD diagram of the lithium product obtained by evaporation and crystallization in Example 1;

[0022] Figure 5 This is the XRD diagram of the manganese product obtained by evaporation and crystallization in Example 1. DETAILED DESCRIPTION

[0023] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0024] As used herein, the term "prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0025] When amount, concentration or other value or parameter is expressed as range, preferred range or a series of upper preferred value and lower preferred value limit range, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value and any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when disclosing range "1 to 5", described range should be interpreted as including range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the range is intended to include its end value and all integers and fractions within the range.

[0026] In addition, the indefinite articles "a" and "an" before the elements or components of the present invention have no restrictions on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the number is obviously intended to be in the singular form.

[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0028] A method for recovering valuable metals in a co-baked product of retired lithium iron phosphate and a ternary positive electrode material comprises the following steps:

[0029] S1: The retired lithium iron phosphate and the ternary positive electrode material are uniformly mixed in a molar ratio of 1.5:1, and then placed in a tubular furnace under nitrogen protection for 1.5 hours of calcination at a temperature of 600°C to obtain a co-calcined product; the ternary positive electrode material is one or a mixture of NCM111, NCM523, NCM622, and NCM811 materials; the co-calcined product obtained is mainly: lithium phosphate, nickel monoxide, cobalt monoxide, nickel cobalt element, manganese monoxide and ferroferric oxide.

[0030] S2: placing the obtained co-calcined product in a (NH4)2SO4-NH3·H2O system for ammonia leaching reaction, and selectively leaching lithium, nickel and cobalt elements; the (NH4)2SO4-NH3·H2O system has a (NH4)2SO4 concentration of 1-3 mol / L, a NH3·H2O concentration of 2-4 mol / L, a solid-liquid ratio of 5-20 g / L, a leaching temperature of the ammonia leaching reaction of 60-120°C, and ammonia leaching time of 1-3 h.

[0031] S3: After the ammonia leaching is completed, the ammonia leaching solution containing lithium, nickel and cobalt ions and the ammonia leaching residue containing manganese and iron elements are obtained by solid-liquid separation;

[0032] S4: introducing an electrolytic cell having a titanium-based ruthenium-iridium oxide coating electrode as an anode and a titanium plate as a cathode into the ammonia immersion solution;

[0033] S5: Electrodepositing nickel ions and cobalt ions in an ammonia immersion solution in an electrolytic cell by an electrochemical deposition method and recovering them in the form of an alloy, and then evaporating and crystallizing the remaining lithium element in the electrodeposition residual solution to obtain a Li(NH4)(SO4) product; the voltage in the electrochemical deposition method is 4-8V, and the electrolysis is performed at room temperature for 3-9h; since nickel and cobalt ions form a complex with ammonium ions, the oxidation of the anode during the electrodeposition process can break the coordination structure of the complex, release metal ions and free ammonia, and promote the reduction deposition and recovery of nickel and cobalt ions at the cathode.

[0034] S6: The manganese in the ammonia leached slag is subjected to water leaching to obtain an iron slag product and a manganese-containing solution, and the obtained manganese-containing solution is subjected to evaporation and crystallization to obtain a (NH4)2Mn(SO4)2·6H2O product; the solid-liquid ratio in the water leaching method is 50-150g / L, the temperature is 25-90°C, and the reaction time is 0.5h.

[0035] It should be noted that the lithium, nickel and cobalt elements in the co-baked product can be selectively leached through the (NH4)2SO4-NH3·H2O system, effectively avoiding too many types of metal ions from entering the electrochemical reaction system to interfere with the co-deposition of the target metal. Since the ammonium ions in the ammonia leaching process have a complexing effect on nickel and cobalt ions, the conventional precipitation method has a poor precipitation effect or still needs to add a certain amount of complex breaking reagent. The present invention breaks the coordination structure of the complex through an electrochemical anode reaction and simultaneously realizes the co-deposition of nickel and cobalt ions at the cathode; at the same time, the ammonia in the solution assists the electrodeposition to obtain a uniform nickel and cobalt alloy deposition product; the lithium resources in the residual solution of the electrodeposition can be obtained by simple evaporation and crystallization to obtain the Li(NH4)(SO4) product.

[0036] In addition, in step S6, in the ammonia leaching residue, manganese and iron elements exist in the form of (NH4)2Mn(SO4)2 and Fe3O4, respectively. By utilizing the property that (NH4)2Mn(SO4)2 is easily soluble in water, manganese resources can be recovered from the ammonia leaching residue by simple water leaching. After the water leaching is completed and filtered, an iron slag product and a manganese-containing solution are obtained; the manganese-containing solution is evaporated and crystallized to obtain a manganese product.

[0037] Example 1

[0038] A method for recovering valuable metals in a co-baked product of retired lithium iron phosphate and a ternary positive electrode material comprises the following steps:

[0039] S1: The retired lithium iron phosphate and NCM111 ternary positive electrode materials are uniformly mixed in a molar ratio of 1.5:1 and placed in a tubular furnace under nitrogen protection for calcination for 1.5 hours at a calcination temperature of 600°C to obtain a co-calcined product; the co-calcined product obtained is mainly: lithium phosphate, nickel monoxide, cobalt monoxide, nickel cobalt element, manganese monoxide and ferrosoferric oxide.

[0040] S2: The product of the co-calcination of retired lithium iron phosphate and NCM111 ternary positive electrode material is placed in an ammonia leaching reaction vessel, and reacted for 1 hour under the conditions of an initial concentration of 1 mol / L (NH4)2SO4 and 4 mol / L NH3·H2O, a solid-liquid ratio of 20 g / L, and an ammonia leaching temperature of 120°C. The selective leaching efficiencies of lithium, nickel, and cobalt elements are 99.27%, 99.16%, and 99.11%, respectively, achieved by the complexation of ammonium ions. The XRD results of the ammonia leaching residue of the co-calcination product of retired lithium iron phosphate and ternary positive electrode material are shown in the figure. Figure 2 shown.

[0041] S3: After the ammonia leaching is completed, the ammonia leaching solution containing lithium, nickel and cobalt ions and the ammonia leaching residue containing manganese and iron elements are obtained by solid-liquid separation;

[0042] S4: introducing an electrolytic cell having a titanium-based ruthenium-iridium oxide coating electrode as an anode and a titanium plate as a cathode into the ammonia immersion solution;

[0043] S5: Electrochemically deposit the nickel ions and cobalt ions in the ammonia immersion solution in the electrolytic cell and recover them in the form of an alloy, and then evaporate and crystallize the remaining lithium in the electrodeposition solution to obtain the Li(NH4)(SO4) product; co-deposit the nickel ions and cobalt ions at 4V for 9 hours, and recover 99.15% of the nickel and 99.24% of the cobalt in the form of an alloy. The SEM-EDS results of the nickel-cobalt alloy recovered by electrochemical co-deposition are as follows: Figure 3 As shown; the XRD results of the evaporated crystallized lithium product are as follows Figure 4 shown.

[0044] S6: The manganese in the ammonia leaching residue is leached in water to obtain an iron slag product and a manganese-containing solution. The obtained manganese-containing solution is evaporated and crystallized to obtain a (NH4)2Mn(SO4)2·6H2O product. In the ammonia leaching residue, manganese and iron elements exist in the form of (NH4)2Mn(SO4)2 and Fe3O4, respectively. By utilizing the property that (NH4)2Mn(SO4)2 is easily soluble in water, 99.24% of the manganese resources can be recovered from the ammonia leaching residue by immersing in water at a solid-liquid ratio of 50g / L and a temperature of 25°C for 0.5h. After immersion, the iron slag product and the manganese-containing solution are obtained by filtration. The manganese-containing solution is evaporated and crystallized to obtain a (NH4)2Mn(SO4)2·6H2O product. The XRD results of the manganese product recovered by evaporation and crystallization are as follows: Figure 5shown.

[0045] Example 2

[0046] A method for recovering valuable metals in a co-baked product of retired lithium iron phosphate and a ternary positive electrode material comprises the following steps:

[0047] S1: The retired lithium iron phosphate and NCM523 ternary cathode material were uniformly mixed at a molar ratio of 1.5:1 and placed in a tubular furnace under nitrogen protection for 1.5 hours of calcination at a calcination temperature of 600°C to obtain a co-calcined product;

[0048] S2: The co-calcined product of retired lithium iron phosphate and NCM523 ternary positive electrode material is placed in an ammonia leaching reaction vessel, and reacted for 2 hours under the conditions of initial concentration of 2 mol / L (NH4)2SO4 and 3 mol / L NH3·H2O, solid-liquid ratio of 10 g / L and ammonia leaching temperature of 90°C. Relying on the complexation of ammonium ions, the selective leaching efficiencies of lithium, nickel and cobalt elements are 99.51%, 99.47% and 99.38% respectively.

[0049] S3: After the ammonia leaching is completed, the ammonia leaching solution containing lithium, nickel and cobalt ions and the ammonia leaching residue containing manganese and iron elements are obtained by solid-liquid separation;

[0050] S4: introducing an electrolytic cell having a titanium-based ruthenium-iridium oxide coating electrode as an anode and a titanium plate as a cathode into the ammonia immersion solution;

[0051] S5: The nickel ions and cobalt ions in the ammonia immersion solution are electrochemically deposited in an electrolytic cell and recovered in the form of an alloy, and the lithium element remaining in the electrodeposition residual solution is evaporated and crystallized to obtain a Li(NH4)(SO4) product; after the nickel ions and cobalt ions are co-deposited at a voltage of 6V for 6 hours, 99.27% ​​of the nickel and 99.13% of the cobalt are recovered in the form of an alloy.

[0052] S6: The manganese in the ammonia leached residue is subjected to water leaching to obtain an iron slag product and a manganese-containing solution, and the obtained manganese-containing solution is subjected to evaporation and crystallization to obtain a (NH4)2Mn(SO4)2·6H2O product; in the ammonia leached residue, manganese and iron elements exist in the form of (NH4)2Mn(SO4)2 and Fe3O4, respectively. By utilizing the property that (NH4)2Mn(SO4)2 is easily soluble in water, 99.33% of the manganese resources can be recovered from the ammonia leached residue by water immersion at a solid-liquid ratio of 100 g / L and a temperature of 50°C for 0.5 h. After the water immersion is completed and filtered, the iron slag product and the manganese-containing solution are obtained; the manganese-containing solution is subjected to evaporation and crystallization to obtain the (NH4)2Mn(SO4)2·6H2O product.

[0053] Example 3

[0054] A method for recovering valuable metals in a co-baked product of retired lithium iron phosphate and a ternary positive electrode material comprises the following steps:

[0055] S1: The retired lithium iron phosphate and NCM622+NCM811 ternary cathode materials were uniformly mixed at a molar ratio of 1.5:1 and then placed in a tubular furnace under nitrogen protection for 1.5 hours of calcination at a calcination temperature of 600°C to obtain a co-calcined product;

[0056] S2: The co-calcined product of retired lithium iron phosphate and NCM622+NCM811 ternary positive electrode materials is placed in an ammonia leaching reaction vessel, and reacted for 3 hours under the conditions of an initial concentration of 3 mol / L (NH4)2SO4 and 2 mol / L NH3·H2O, a solid-liquid ratio of 5 g / L and an ammonia leaching temperature of 60°C. Relying on the complexation of ammonium ions, the selective leaching efficiencies of lithium, nickel and cobalt elements are 99.65%, 99.49% and 99.46%, respectively.

[0057] S3: After the ammonia leaching is completed, the ammonia leaching solution containing lithium, nickel and cobalt ions and the ammonia leaching residue containing manganese and iron elements are obtained by solid-liquid separation;

[0058] S4: introducing an electrolytic cell having a titanium-based ruthenium-iridium oxide coating electrode as an anode and a titanium plate as a cathode into the ammonia immersion solution;

[0059] S5: The nickel ions and cobalt ions in the ammonia immersion solution are electrochemically deposited in an electrolytic cell and recovered in the form of an alloy, and the lithium element remaining in the electrodeposition residual solution is evaporated and crystallized to obtain a Li(NH4)(SO4) product; after the nickel ions and cobalt ions are co-deposited at a voltage of 8V for 3 hours, 99.34% of the nickel and 99.28% of the cobalt are recovered in the form of an alloy.

[0060] S6: The manganese in the ammonia leached residue is subjected to water leaching to obtain an iron slag product and a manganese-containing solution, and the obtained manganese-containing solution is subjected to evaporation and crystallization to obtain a (NH4)2Mn(SO4)2·6H2O product; in the ammonia leached residue, manganese and iron elements exist in the form of (NH4)2Mn(SO4)2 and Fe3O4, respectively. By utilizing the property that (NH4)2Mn(SO4)2 is easily soluble in water, 99.41% of the manganese resources can be recovered from the ammonia leached residue by water immersion at a solid-liquid ratio of 150g / L and a temperature of 90°C for 0.5h. After the water immersion is completed and filtered, the iron slag product and the manganese-containing solution are obtained; the manganese-containing solution is subjected to evaporation and crystallization to obtain the (NH4)2Mn(SO4)2·6H2O product.

[0061] The above-mentioned method for recovering valuable metals in the co-roasting products of retired lithium iron phosphate and ternary positive electrode materials is highly targeted and easy to implement. It provides a simple and efficient idea for the recovery of multi-electrode material blends in the process of large-scale lithium-ion battery resource utilization, and realizes the efficient resource utilization of multiple metals in the co-roasting products of retired lithium iron phosphate and ternary positive electrode materials.

[0062] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0063] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for recovering valuable metals from the co-baking product of retired lithium iron phosphate and ternary positive electrode materials, It is characterized in that The following steps are involved: S1: The retired lithium iron phosphate and the ternary cathode material are uniformly mixed at a molar ratio of 1.5:1 and then placed in a tubular furnace under nitrogen protection for 1.5 hours of calcination at a calcination temperature of 600°C to obtain a co-calcined product; S2: placing the obtained co-calcined product in a (NH4)2SO4-NH3·H2O system for ammonia leaching reaction, and selectively leaching lithium, nickel and cobalt elements; S3: After the ammonia leaching is completed, the ammonia leaching solution containing lithium, nickel and cobalt ions and the ammonia leaching residue containing manganese and iron elements are obtained by solid-liquid separation; S4: introducing an electrolytic cell having a titanium-based ruthenium-iridium oxide coating electrode as an anode and a titanium plate as a cathode into the ammonia immersion solution; S5: Electrodepositing nickel ions and cobalt ions in the ammonia immersion solution in an electrolytic cell by an electrochemical deposition method and recovering them in the form of an alloy, and then evaporating and crystallizing the lithium element remaining in the electrodeposition residual solution to obtain a Li(NH4)(SO4) product; S6: The manganese in the ammonia leached slag is leached in water to obtain an iron slag product and a manganese-containing solution, and the obtained manganese-containing solution is evaporated and crystallized to obtain a (NH4)2Mn(SO4)2·6H2O product.

2. A method for recovering valuable metals in a co-baked product of retired lithium iron phosphate and ternary positive electrode materials according to claim 1, It is characterized in that In step S1, the ternary positive electrode material is one or a mixture of NCM111, NCM523, NCM622, and NCM811.

3. A method for recovering valuable metals in a co-baked product of retired lithium iron phosphate and ternary positive electrode materials according to claim 1, It is characterized in that In step S2, the (NH4)2SO4 concentration in the (NH4)2SO4-NH3·H2O system is 1-3 mol / L, the NH3·H2O concentration is 2-4 mol / L, the solid-liquid ratio is 5-20 g / L, the leaching temperature of the ammonia leaching reaction is 60-120°C, and the ammonia leaching time is 1-3 h.

4. A method for recovering valuable metals in a co-baked product of retired lithium iron phosphate and ternary positive electrode materials according to claim 1, It is characterized in that In step S5, the voltage in the electrochemical deposition method is 4-8V, and the electrolysis is performed at room temperature for 3-9 hours.

5. A method for recovering valuable metals in a co-baked product of retired lithium iron phosphate and ternary positive electrode materials according to claim 1, It is characterized in that In step S6, the solid-liquid ratio in the water immersion method is 50-150 g / L, the temperature is 25-90° C., and the reaction time is 0.5 h.

Citation Information

Patent Citations

  • Method for preparing olivine type five-element high-entropy lithium battery precursor by recycling lithium battery

    CN112093787A

  • Method for recycling valuable metals from waste lithium ion batteries

    CN117845057A

  • Method for treating mixed waste lithium battery through autocatalytic reaction and regenerating nickel-cobalt-manganese ternary lithium battery

    CN118352679A

  • Method for recovering metal from positive electrode material for lithium ion batteries

    JP2015103320A

  • Treatment method of positive electrode active substance waste product of lithium ion secondary battery

    WO2020090690A1