Method for selectively extracting and separating germanium by using quaternary ammonium salt extracting agent
By using quaternary ammonium salt extractant in high-ferroal high-alumina sulfuric acid-organic acid solution, germanium residue is treated with sulfuric acid and organic acid, and combined with quaternary ammonium salt extractant, the efficient separation of germanium and impurity elements is achieved, and the existing solution is solved The germanium recycling method in the technology has high cost, complex process and environmental pollution problems, achieving efficient and environmentally friendly germanium extraction effect.
Patent Information
- Application Number
- CN202411046874.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-29
AI Technical Summary
In the existing germanium recovery methods, the tannin precipitation method is costly, the impurity co-precipitation, the ion exchange method is complex and the production cycle is long. The solvent extraction method requires high alkalinity during the back extraction process, which affects the environment; and in high-iron high-alumina sulfuric acid -It is difficult to separate germanium and impurity elements in organic acid solutions.
Using quaternary ammonium salt extractant, leaching the germanium residue through sulfuric acid and organic acid, mixing quaternary ammonium salt, regulator and diluent to form an extracted organic phase and an acidic leaching liquid as an aqueous phase. After shock and back-extraction treatment, germanium and Selective separation of impurities such as iron, aluminum, zinc, nickel, copper, arsenic and other impurities.
It realizes efficient selective extraction and separation of germanium in high-iron high-alumina sulfuric acid-organic acid solution, reduces the use of alkaline solution, extends the service life of the extractant, reduces environmental pollution, and has a high extraction rate and impurity element extraction rate. Close to 0.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of hydrometallurgy, and specifically relates to a method for selectively extracting and separating germanium using a quaternary ammonium salt extractant. Background Art
[0002] Germanium is a rare metal element with important strategic value. Due to its unique semiconductor and optical properties, it is widely used in the preparation of infrared equipment, optical fiber materials, polymer catalysts and solar panels. However, germanium is often associated with minerals such as non-ferrous metals and rarely exists in the form of a single mineral. This results in the extraction of iron, aluminum and other impurity ions during the extraction of germanium. Therefore, it is very important to study how to selectively separate germanium from a large number of associated elements.
[0003] At present, the most common methods for recovering germanium in hydrometallurgy are tannin precipitation, solvent extraction, ion exchange, etc. Among them, tannin precipitation has the disadvantages of large amount of tannic acid and high cost, and impurity metals are easy to co-precipitate. The ion exchange method for extracting germanium has a complicated process flow, large infrastructure investment, long production cycle, and cannot be put into actual production on a large scale. Solvent extraction has the advantages of fast equilibrium speed, strong selectivity, and relatively simple process flow, making it the preferred method for recovering germanium.
[0004] The hydroxyoxime extractant Lix-63 requires a higher alkalinity during stripping, which reduces the service life of the extractant. In high-arsenic and high-silicon sulfate solutions, it is difficult to separate germanium and arsenic. Kelex100 extracts germanium with good selectivity for cadmium, zinc, cobalt, and nickel, but poor selectivity for copper and iron. The N235-TBP system also requires a higher alkali concentration during stripping when extracting germanium. A large amount of acid will be consumed in the subsequent germanium hydrolysis process, causing damage to the environment. Summary of the invention
[0005] The purpose of the present application is to overcome the deficiencies of the prior art and provide a method for selectively extracting and separating germanium using a quaternary ammonium salt extractant, selectively extracting and separating germanium from a high-iron and high-aluminum sulfuric acid-organic acid solution, and achieving efficient separation of germanium from impurity elements such as iron, aluminum, zinc, and arsenic.
[0006] The technical problem solved by this application is achieved through the following technical solutions:
[0007] A method for selectively extracting and separating germanium using a quaternary ammonium salt extractant, the method comprising the following steps:
[0008] S1, using sulfuric acid and organic acid to leaching germanium slag to obtain germanium-containing acidic leaching solution;
[0009] S2, adjusting the volume of the above germanium-containing acidic leaching solution to serve as an extraction water phase;
[0010] S3, mixing the quaternary ammonium salt, the regulator, the co-solvent and the diluent in a certain proportion to form an extraction organic phase;
[0011] S4, mixing the above-mentioned extracted organic phase and the extracted aqueous phase and shaking them fully to obtain a loaded organic phase containing germanium and an aqueous phase containing a small amount of germanium and impurity ions of iron, aluminum, nickel, copper, zinc and arsenic;
[0012] S5. Use an alkaline solution and fully mix it with the loaded organic phase to perform organic back extraction to obtain a pure germanium-containing back extraction solution.
[0013] Moreover, the concentration of sulfuric acid used in S1 is 10% to 30%; the organic acid in S1 is one of citric acid, salicylic acid, tartaric acid, and catechol;
[0014] Optionally, the concentration of tartaric acid is 5% to 20%, and the concentration of germanium ions in the germanium-containing acidic leaching solution is 0.1 to 0.45 g / L.
[0015] Moreover, the pH of the extracted aqueous phase of S2 is 0.1-5.
[0016] Moreover, the iron ion concentration of the S2 extracted water phase is 0.1-3.6 g / L, the zinc ion concentration is 0.1-1.4 g / L, the aluminum ion concentration is 0.1-1 g / L, the nickel ion concentration is 0.1-0.7 g / L, the copper ion concentration is 0.1-0.2 g / L, and the arsenic ion concentration is 0.1-0.4 g / L.
[0017] Moreover, the quaternary ammonium salt used in S3 is compound I, and the chemical general formula I of the quaternary ammonium salt is:
[0018]
[0019] Wherein, n is an integer from 0 to 5;
[0020] Substituent R 1 , R 2 and R 3 Each independently represents any one of an alkyl group, an alkenyl group, an alkynyl group having 1 to 30 carbon atoms, and an aromatic group having 6 to 30 carbon atoms, and X represents a halogen element.
[0021] Moreover, the diluent of S3 is one of sulfonated kerosene, carbon tetrachloride, toluene, chlorobenzene or chloroform, the regulator is TBP or TOP, and the cosolvent is isooctyl alcohol or sec-octanol.
[0022] Moreover, the weight ratio of the diluent: the regulator: the cosolvent: the quaternary ammonium salt in S3 is (1-500): (1-200): (1-100): (1-50).
[0023] Moreover, the mass ratio of the aqueous phase to the organic phase in S4 is (1:9) to (9:1), the shaking stirring time is 1 to 100 minutes, the stirring temperature is 25 to 50° C., and the extraction level is 1 to 5.
[0024] Moreover, the S5 alkaline solution is ammonia water or sodium hydroxide solution, and the optional concentration of the sodium hydroxide solution is 0.08-2 mol / L.
[0025] Moreover, the mass ratio of the stripping water phase and the organic phase of the S5 organic back-extraction is (1:9) to (9:1), the stirring time is 1 to 100 minutes, the stirring temperature is 25 to 50° C., and the back-extraction level is 1 to 5.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1. The germanium extraction process adopted in the present invention can selectively extract and separate germanium in a high-iron and high-aluminum sulfuric acid-organic acid solution. The extraction process has a high extraction rate for germanium, and the extraction rate for elements such as iron, aluminum, zinc, nickel, arsenic, and copper is close to 0.
[0028] 2. Compared with common phosphoric acid extractants, the extractant used in the present invention does not require saponification and can be directly used for extraction without generating a large amount of salt-containing and ammonia-containing wastewater.
[0029] 3. The germanium extraction process adopted by the present invention reduces the use of alkaline solution in the pH adjustment link of the extraction mother liquor. At the same time, the extractant can be reused after the back extraction stage, which effectively prolongs the service life of the extractant and plays a positive role in the comprehensive recovery and utilization of germanium. DETAILED DESCRIPTION
[0030] The present application is further described in detail below through specific examples. The following examples are only descriptive and not restrictive, and the protection scope of the present application cannot be limited by them.
[0031] A method for selectively extracting and separating germanium using a quaternary ammonium salt extractant, the innovation of which lies in the steps of:
[0032] S1, using sulfuric acid and organic acid to leaching germanium slag to obtain germanium-containing acidic leaching solution;
[0033] S2, adjusting the volume of the above germanium-containing acidic leaching solution to serve as an extraction water phase;
[0034] S3, mixing the quaternary ammonium salt, the regulator, the co-solvent and the diluent in a certain proportion to form an extraction organic phase;
[0035] S4, mixing the above-mentioned extracted organic phase and the extracted aqueous phase and shaking them fully to obtain a loaded organic phase containing germanium and an aqueous phase containing a small amount of germanium and impurity ions of iron, aluminum, nickel, copper, zinc and arsenic;
[0036] S5. Use an alkaline solution and fully mix it with the loaded organic phase to perform organic back extraction to obtain a pure germanium-containing back extraction solution.
[0037] Moreover, the concentration of sulfuric acid used in S1 is 10% to 30%; the organic acid in S1 is one of citric acid, salicylic acid, tartaric acid, and catechol;
[0038] Optionally, the concentration of tartaric acid is 5% to 20%, and the concentration of germanium ions in the germanium-containing acidic leaching solution is 0.1 to 0.45 g / L.
[0039] Moreover, the pH of the extracted aqueous phase of S2 is 0.1-5.
[0040] Moreover, the iron ion concentration of the S2 extracted water phase is 0.1-3.6 g / L, the zinc ion concentration is 0.1-1.4 g / L, the aluminum ion concentration is 0.1-1 g / L, the nickel ion concentration is 0.1-0.7 g / L, the copper ion concentration is 0.1-0.2 g / L, and the arsenic ion concentration is 0.1-0.4 g / L.
[0041] Moreover, the quaternary ammonium salt used in S3 is compound I, and the chemical general formula I of the quaternary ammonium salt is:
[0042]
[0043] Wherein, n is an integer from 0 to 5;
[0044] Substituent R 1 , R 2 and R 3 Each independently represents any one of an alkyl group, an alkenyl group, an alkynyl group having 1 to 30 carbon atoms, and an aromatic group having 6 to 30 carbon atoms, and X represents a halogen element.
[0045] Moreover, the diluent of S3 is one of sulfonated kerosene, carbon tetrachloride, toluene, chlorobenzene or chloroform, the regulator is TBP or TOP, and the cosolvent is isooctyl alcohol or sec-octanol.
[0046] Moreover, the weight ratio of the diluent: the regulator: the cosolvent: the quaternary ammonium salt in S3 is (1-500): (1-200): (1-100): (1-50).
[0047] Moreover, the mass ratio of the aqueous phase to the organic phase in S4 is (1:9) to (9:1), the shaking stirring time is 1 to 100 minutes, the stirring temperature is 25 to 50° C., and the extraction level is 1 to 5.
[0048] Moreover, the S5 alkaline solution is ammonia water or sodium hydroxide solution, and the optional concentration of the sodium hydroxide solution is 0.08-2 mol / L.
[0049] Moreover, the mass ratio of the stripping water phase and the organic phase of the S5 organic back-extraction is (1:9) to (9:1), the stirring time is 1 to 100 minutes, the stirring temperature is 25 to 50° C., and the back-extraction level is 1 to 5.
[0050] The testing method of the present invention:
[0051] The extraction solution, raffinate and stripping solution were diluted 2500 times to prepare the test sample. The diluted aqueous metal ions were detected by ICP-MS (Inductively Coupled Plasma Mass Spectrometry), which is called inductively coupled plasma mass spectrometry in Chinese. ICP-MS consists of an ICP torch, a mass spectrometer and an interface device, and mainly relies on the analysis and calculation of the mass spectrometer. The ICP torch is responsible for generating high-temperature plasma, which ionizes the gas through high-voltage electric sparks and generates plasma gas flow through high-frequency electric fields, and forms a stable plasma torch at the nozzle through the push of the gas. The test sample is atomized in the system to form an aerosol, which is brought into the central area of the isoflurane torch by the carrier gas. The aerosol is evaporated, decomposed, excited and ionized to produce ions. The interface composed of a sampling cone and a skimmer cone transmits the ions to the mass spectrometer, which separates the charged ions according to the mass-to-charge ratio (m / z), thereby analyzing and calculating the intensity of the elements.
[0052] The samples were analyzed using an inductively coupled plasma mass spectrometer (ICP-MS) of model ICAP RQ (manufactured by Thermo Fisher Scientific Inc.).
[0053] Data processing:
[0054] Extraction rate (E): The extraction rate is used to indicate the completeness of the extraction of the extracted substance from the aqueous phase to the organic phase, that is, the ratio of the content of the extracted substance in the organic phase after extraction to the content in the initial aqueous phase. It can be directly obtained after measurement and can directly reflect the extraction effect. It is calculated by formula (1):
[0055]
[0056] Where:
[0057] E—extraction rate, %
[0058] C o —Initial metal concentration in aqueous phase before extraction, mg / L
[0059] C e —Metal concentration in aqueous phase after extraction, mg / L
[0060] Distribution ratio (D): When separating and purifying substances by solvent extraction, it is used to indicate the ease with which the substance is extracted and separated. It is obtained by analyzing the distribution relationship of the substance in the two phases after extraction, that is, the ratio of the concentration of the extracted substance in the organic phase to the concentration in the aqueous phase, calculated by formula (2).
[0061]
[0062] Where:
[0063] D—Distribution ratio
[0064] C o —Initial metal concentration in aqueous phase before extraction, mg / L
[0065] C e —Metal concentration in aqueous phase after extraction, mg / L
[0066] V aq —The volume of the aqueous phase in the extraction system, L
[0067] V org —The volume of the organic phase in the extraction system, L
[0068] Stripping rate (S): when stripping the target substance from the loaded organic phase, it is used to indicate the completeness of the stripping of the target substance into the aqueous phase, that is, the ratio of the content of the loaded organic phase substance to the content of the aqueous phase substance after stripping, calculated by formula (3).
[0069]
[0070] Where:
[0071] S—stripping rate, %
[0072] M aq —Content of aqueous phase after stripping, mg
[0073] M org —Content of organic phase loaded, mg
[0074] Separation coefficient (β): If there are other components in the extraction system besides the substance to be extracted and separated, the separation coefficient can be used to measure the difficulty of separating them by extraction. The larger the value, the easier it is to extract and separate the two. It is the ratio of the distribution ratios of the two substances to be separated and is calculated by formula (4).
[0075]
[0076] Where:
[0077] β Ge / Me —Separation coefficient of germanium and impurity ions
[0078] D Ge— Distribution ratio of germanium
[0079] D Me —Distribution ratio of impurity ions.
[0080] Example 1
[0081] (1) 1 g of germanium slag and 3 g of mixed acid solution (15% sulfuric acid and 5% tartaric acid) were stirred at 120° C. for 4 h to obtain a germanium leaching solution;
[0082] (2) The germanium leaching solution was diluted to a 20 mL volumetric flask to obtain an aqueous extraction phase with a pH of 0.74;
[0083] (3) 2 g of sulfonated kerosene, 2.5 g of TBP, 0.5 g of isooctyl alcohol, and 0.16 g of quaternary ammonium salt were fully mixed to prepare an organic phase;
[0084] (4) 20 g of the aqueous phase and 5 g of the organic phase were mixed, and stirred at a speed of 500 r / min for 2 min using a magnetic stirrer at a stirring temperature of 25° C., thereby obtaining an organic phase rich in most of the germanium in the pre-extraction solution and an aqueous phase containing a small amount of germanium and impurity ions such as iron, aluminum, magnesium, nickel, copper, zinc, and arsenic. The 20 g of the aqueous phase obtained after the above extraction was mixed with 5 g of the fresh aqueous phase, and the organic phases obtained from the two times were mixed to obtain a stripping organic phase. After extraction equilibrium, the extraction rate of germanium was 94.47%, and the extraction separation coefficients of the impurity metals are shown in Table 1.
[0085] (5) 10 g of the loaded organic phase and 20 g of 0.3 M sodium hydroxide stripping solution were mixed, and stirred at a speed of 500 r / min for 2 min using a magnetic stirrer. The stirring temperature was 25° C. After stripping equilibrium, the germanium stripping rate could reach more than 95%. A pure germanium-containing stripping solution could be obtained after one stripping.
[0086] Table 1 Extraction and separation coefficients of metal impurities in liquid feed
[0087] Element ratio Ge / Fe Ge / Al Ge / As Ge / Cu Ge / Zn Ge / Ni divisional number β 1195207.1 1792819.7 6721.1 1379087.9 1379087.9 1494013.4
[0088] Example 2
[0089] (1) 1 g of germanium slag and 3 g of mixed acid solution (15% sulfuric acid and 5% tartaric acid) were stirred at 120° C. for 4 h to obtain a germanium leaching solution.
[0090] (2) The germanium leaching solution was diluted to a 20 mL volumetric flask, and the pH of the solution was adjusted using a 10 M sodium hydroxide solution to obtain an aqueous extraction phase with a pH of 1.
[0091] (3) 2 g of sulfonated kerosene, 2.5 g of TBP, 0.5 g of isooctyl alcohol, and 0.16 g of quaternary ammonium salt were thoroughly mixed to prepare an organic phase.
[0092] (4) 20 g of the aqueous phase and 5 g of the organic phase were mixed, and stirred at a speed of 500 r / min for 2 min using a magnetic stirrer at a stirring temperature of 25° C., thereby obtaining an organic phase rich in most of the germanium in the pre-extraction solution and an aqueous phase containing a small amount of germanium and impurity ions such as iron, aluminum, magnesium, nickel, copper, zinc, and arsenic. The 20 g of the aqueous phase obtained after the above extraction was mixed with 5 g of the fresh aqueous phase, and the organic phases obtained from the two times were mixed to obtain a stripping organic phase. After extraction equilibrium, the extraction rate of germanium was 85.26%. The extraction separation coefficients of the impurity metals are shown in Table 2.
[0093] (5) 10 g of the loaded organic phase and 20 g of 0.3 M sodium hydroxide stripping solution were mixed, and stirred at a speed of 500 r / min for 2 min using a magnetic stirrer. The stirring temperature was 25° C. After stripping equilibrium, the germanium stripping rate could reach more than 95%. A pure germanium-containing stripping solution could be obtained after one stripping.
[0094] Table 2 Extraction and separation coefficients of metal impurities in liquid feed
[0095] Element ratio Ge / Fe Ge / Al Ge / As Ge / Cu Ge / Zn Ge / Ni divisional number β 150769.2 417.1 217.8 3266.7 178181.8 115294.1
[0096] Example 3
[0097] (1) 1 g of germanium slag and 3 g of mixed acid solution (15% sulfuric acid and 5% tartaric acid) were stirred at 120° C. for 4 h to obtain a germanium leaching solution.
[0098] (2) The germanium leaching solution is diluted to a 20 mL volumetric flask to obtain an extraction aqueous phase with a pH of 0.74.
[0099] (3) 2 g of sulfonated kerosene, 2.5 g of TBP, 0.5 g of isooctyl alcohol, and 0.08 g of quaternary ammonium salt were thoroughly mixed to prepare an organic phase.
[0100] (4) 20 g of the aqueous phase and 5 g of the organic phase were mixed, and stirred at a speed of 500 r / min for 2 min using a magnetic stirrer at a stirring temperature of 25° C., thereby obtaining an organic phase rich in most of the germanium in the pre-extraction solution and an aqueous phase containing a small amount of germanium and impurity ions such as iron, aluminum, magnesium, nickel, copper, zinc, and arsenic. The 20 g of the aqueous phase obtained after the above extraction was mixed with 5 g of the fresh aqueous phase, and the organic phases obtained from the two times were mixed to obtain a stripping organic phase. After extraction equilibrium, the extraction rate of germanium was 79.18%, and the extraction separation coefficients of the impurity metals were shown in Table 3.
[0101] (5) 10 g of the loaded organic phase and 20 g of 0.3 M sodium hydroxide stripping solution were mixed, and stirred at a speed of 500 r / min for 2 min using a magnetic stirrer. The stirring temperature was 25° C. After stripping equilibrium, the germanium stripping rate could reach more than 95%. A pure germanium-containing stripping solution could be obtained after one stripping.
[0102] Table 3 Extraction separation coefficient of impurities and metals in liquid feed
[0103] Element ratio Ge / Fe Ge / Al Ge / As Ge / Cu Ge / Zn Ge / Ni divisional number β 39948.7 1378.76 66.58 43764.1 2605.4 37095.2
[0104] Example 4
[0105] (1) 1 g of germanium slag and 3 g of mixed acid solution (15% sulfuric acid and 5% tartaric acid) were stirred at 120° C. for 4 h to obtain a germanium leaching solution.
[0106] (2) The germanium leaching solution was diluted to a 20 mL volumetric flask, and the pH was adjusted using a 10 M sodium hydroxide solution to obtain an aqueous extraction phase with a pH of 1.5.
[0107] (3) 2 g of sulfonated kerosene, 2.5 g of TBP, 0.5 g of isooctyl alcohol, and 0.16 g of quaternary ammonium salt were thoroughly mixed to prepare an organic phase.
[0108] (4) 20 g of the aqueous phase and 5 g of the organic phase were mixed, and stirred at a speed of 500 r / min for 2 min using a magnetic stirrer at a stirring temperature of 25° C., thereby obtaining an organic phase rich in most of the germanium in the pre-extraction solution and an aqueous phase containing a small amount of germanium and impurity ions such as iron, aluminum, magnesium, nickel, copper, zinc, and arsenic. The 20 g of the aqueous phase obtained after the above extraction was mixed with 5 g of the fresh aqueous phase, and the organic phases obtained from the two times were mixed to obtain a stripping organic phase. After extraction equilibrium, the extraction rate of germanium was 79.18%, and the extraction separation coefficients of the impurity metals were shown in Table 4.
[0109] (5) 10 g of the loaded organic phase and 20 g of 0.3 M sodium hydroxide stripping solution were mixed, and stirred at a speed of 500 r / min for 2 min using a magnetic stirrer. The stirring temperature was 25° C. After stripping equilibrium, the germanium stripping rate could reach more than 95%. A pure germanium-containing stripping solution could be obtained after one stripping.
[0110] Table 4 Extraction separation coefficient of impurities and metals in liquid feed
[0111] Element ratio Ge / Fe Ge / Al Ge / As Ge / Cu Ge / Zn Ge / Ni divisional number β 5.5 26.0 0.8 25.4 34.1 32.0
[0112] Example 5
[0113] (1) 1 g of germanium slag and 3 g of mixed acid solution (15% sulfuric acid and 5% tartaric acid) were stirred at 120° C. for 4 h to obtain a germanium leaching solution.
[0114] (2) The germanium leaching solution was diluted to a 20 mL volumetric flask, and the pH of the solution was adjusted with concentrated sulfuric acid to obtain an aqueous extraction phase with a pH of 0.5.
[0115] (3) 2 g of sulfonated kerosene, 2.5 g of TBP, 0.5 g of isooctyl alcohol, and 0.16 g of quaternary ammonium salt were thoroughly mixed to prepare an organic phase.
[0116] (4) 20 g of the aqueous phase and 5 g of the organic phase were mixed, and stirred at a speed of 500 r / min for 2 min using a magnetic stirrer at a stirring temperature of 25° C., thereby obtaining an organic phase rich in most of the germanium in the pre-extraction solution and an aqueous phase containing a small amount of germanium and impurity ions such as iron, aluminum, magnesium, nickel, copper, zinc, and arsenic. The 20 g of the aqueous phase obtained after the above extraction was mixed with 5 g of the fresh aqueous phase, and the organic phases obtained from the two times were mixed to obtain a stripping organic phase. After extraction equilibrium, the extraction rate of germanium was 53.72%. The extraction separation coefficients of the impurity metals are shown in Table 5.
[0117] (5) 10 g of the loaded organic phase and 20 g of 0.3 M sodium hydroxide stripping solution were mixed, and stirred at a speed of 500 r / min for 2 min using a magnetic stirrer. The stirring temperature was 25° C. After stripping equilibrium, the germanium stripping rate could reach more than 95%. A pure germanium-containing stripping solution could be obtained after one stripping.
[0118] Table 5 Extraction and separation coefficients of metal impurities in liquid feed
[0119] Element ratio Ge / Fe Ge / Al Ge / As Ge / Cu Ge / Zn Ge / Ni divisional number β 54112.4 81169.2 4057.4 54112.4 54392.4 57977.7
[0120] Although the embodiments of the present application are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present application and the appended claims. Therefore, the scope of the present application is not limited to the contents disclosed in the embodiments.
Claims
1. A method for selectively extracting and separating germanium using a quaternary ammonium salt extractant, characterized in that: The steps of the method are: S1, using sulfuric acid and organic acid to leaching germanium slag to obtain germanium-containing acidic leaching solution; S2, adjusting the volume of the above germanium-containing acidic leaching solution to serve as an extraction water phase; S3, mixing the quaternary ammonium salt, the regulator, the co-solvent and the diluent in a certain proportion to form an extraction organic phase; S4, mixing the above-mentioned extracted organic phase and the extracted aqueous phase and shaking them fully to obtain a loaded organic phase containing germanium and an aqueous phase containing a small amount of germanium and impurity ions of iron, aluminum, nickel, copper, zinc and arsenic; S5. Use an alkaline solution and fully mix it with the loaded organic phase to perform organic back extraction to obtain a pure germanium-containing back extraction solution.
2. The method for selectively extracting and separating germanium using a quaternary ammonium salt extractant according to claim 1, characterized in that: The concentration of sulfuric acid used in S1 is 10% to 30%; the organic acid in S1 is one of citric acid, salicylic acid, tartaric acid, and catechol; Optionally, the concentration of tartaric acid is 5% to 20%, and the concentration of germanium ions in the germanium-containing acidic leaching solution is 0.1 to 0.45 g / L.
3. The method for selectively extracting and separating germanium using a quaternary ammonium salt extractant according to claim 1, characterized in that: The pH of the extracted aqueous phase of S2 is 0.1-5.
4. The method for selectively extracting and separating germanium using a quaternary ammonium salt extractant according to claim 1, characterized in that: The S2 extracted aqueous phase has an iron ion concentration of 0.1 to 3.6 g / L, a zinc ion concentration of 0.1 to 1.4 g / L, an aluminum ion concentration of 0.1 to 1 g / L, a nickel ion concentration of 0.1 to 0.7 g / L, a copper ion concentration of 0.1 to 0.2 g / L, and an arsenic ion concentration of 0.1 to 0.4 g / L.
5. The method for selectively extracting and separating germanium using a quaternary ammonium salt extractant according to claim 1, characterized in that: The quaternary ammonium salt used in S3 is compound I, and the chemical general formula I of the quaternary ammonium salt is: Wherein, n is an integer from 0 to 5; Substituent R 1 , R 2 and R 3 Each independently represents any one of an alkyl group, an alkenyl group, an alkynyl group having 1 to 30 carbon atoms, and an aromatic group having 6 to 30 carbon atoms, and X represents a halogen element.
6. The method for selectively extracting and separating germanium using a quaternary ammonium salt extractant according to claim 1, characterized in that: The diluent of S3 is one of sulfonated kerosene, carbon tetrachloride, toluene, chlorobenzene or chloroform, the regulator is TBP or TOP, and the cosolvent is isooctyl alcohol or sec-octanol.
7. The method for selectively extracting and separating germanium using a quaternary ammonium salt extractant according to claim 1, characterized in that: The weight ratio of the diluent: the regulator: the co-solvent: the quaternary ammonium salt in S3 is (1-500): (1-200): (1-100): (1-50).
8. The method for selectively extracting and separating germanium using a quaternary ammonium salt extractant according to claim 1, characterized in that: The mass ratio of the aqueous phase to the organic phase in S4 is (1:9) to (9:1), the shaking stirring time is 1 to 100 minutes, the stirring temperature is 25 to 50° C., and the extraction level is 1 to 5.
9. The method for selectively extracting and separating germanium using a quaternary ammonium salt extractant according to claim 1, characterized in that: The S5 alkaline solution is ammonia water or sodium hydroxide solution, and the optional concentration of the sodium hydroxide solution is 0.08-2 mol / L.
10. The method for selectively extracting and separating germanium using a quaternary ammonium salt extractant according to claim 1, characterized in that: The mass ratio of the stripping water phase and the organic phase of the S5 organic back-extraction is (1:9) to (9:1), the stirring time is 1 to 100 minutes, the stirring temperature is 25 to 50° C., and the back-extraction stage is 1 to 5.
Citation Information
Cited By
Method for selectively separating germanium from germanium-rich coal
CN122484506A