Production method of hot-rolled wire rod for low-carbon alloy steel fiber
By adopting specific chemical composition and process flow in the production of low-carbon alloy steel fiber hot-rolled strips, the problems of large fluctuations in tensile strength and uneven tissue are solved, and high-strength and uniform structure of low-carbon alloy steel fiber thermal The production of rolled strips meets the high-quality needs of users.
Patent Information
- Application Number
- CN202411392801.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-11-29
AI Technical Summary
The existing technology is difficult to produce low-carbon alloy steel fiber hot-rolled strips with specifications of Φ5.5mm. The tensile strength fluctuates greatly, the structure is uneven, and the production is difficult, which cannot meet the user's tensile strengths of 550-600MPa and gold. The requirements for the phase structure to be ferrite + pearlite.
Using specific chemical composition and process flows, including continuous casting, rolling, silk spinning and cooling processes, heavy-duty reduce diameter units and 120m-long Steyrmo cooling lines, the chemical composition is controlled to be C: 0.18~0.23%. , Si≤0.10%, Mn: 0.50~0.80%, P≤0.015%, S≤0.010%, Cr: 0.015~0.30%, Ti: 0.03~0.05%, B: 0.0015~0.0040%, by low-temperature rolling and low-temperature Spin and Steyrmo controlled cooling wires to achieve high strength and uniform structure of the strips.
Successfully produced low-carbon alloy steel fiber hot-rolled strips with a hot-rolled tensile strength of 550-600MPa, a grain size of ≥9.0, and a ferrite + pearlite structure, which meets user needs and improves the economic benefits of production and application prospects.
Smart Images

Figure CN119040748A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a production method of a hot-rolled wire rod for low-carbon alloy steel fiber. Background Art
[0002] Steel fiber is mainly used to make steel fiber concrete, which is added to strengthen mortar or concrete. As a new type of material that has appeared in recent years, steel fiber has been increasingly widely used due to its excellent performance in strengthening concrete. With the continuous optimization of production and processing technology and the continuous upgrading of equipment, higher requirements have been placed on the quality of wire rods. The wire rods are required to have small fluctuations in tensile strength, uniform structure, and good pulling performance.
[0003] Patent publication number CN 107177791 B discloses "a hot-rolled wire rod for ultra-low carbon steel fiber and its production method", the chemical composition and mass percentage of the hot-rolled wire rod are: C ≤ 0.010%, Si ≤ 0.03%, Mn ≤ 0.20%, P ≤ 0.020%, S ≤ 0.020%, Alt ≥ 0.02%, Ti: 0.05~
[0004] 0.12%, wherein no boron is added, and the titanium content is also different from that of the present invention, and the cooling method is also different from that of the present invention.
[0005] Patent publication number CN 111690877 A discloses “a method for producing hot-rolled wire rod for ultra-low carbon steel fiber”, whose chemical composition and mass percentage are: C≤0.05wt.%, Si≤0.10wt.%, Mn 0.22~0.35wt.%, S≤0.01wt.%, P≤0.015wt.%, B 0.007~0.009wt.%, Cr≤0.1wt.%, Ni≤0.1wt.%, Cu≤0.1wt.%, Al≤0.01wt.%; Nb 0.02%~0.05wt.%, titanium is not added, and the boron content is also different from that of the present invention.
[0006] After mechanical shelling and descaling, the Φ5.5mm low-carbon alloy steel fiber hot-rolled wire rod is subjected to multiple continuous cold drawing, annealing, and then mechanical shelling and descaling and multiple continuous cold drawing to be processed into Φ0.75mm steel wire. Users require the tensile strength of the Φ5.5mm low-carbon alloy steel fiber hot-rolled wire rod to be controlled between 550-600MPa, with uniform structure and easy mechanical shelling. The existing technical solution is difficult to produce. Summary of the invention
[0007] In order to solve the above technical problems, the present invention provides a production method of hot-rolled wire rod for low-carbon alloy steel fiber, reasonably designs the chemical composition, and utilizes high-speed wire equipment production lines such as heavy-load sizing units and 120m long Stelmor cooling lines to realize the production of hot-rolled wire rod for low-carbon alloy steel fiber, so as to obtain a wire rod with a hot-rolled tensile strength of 550-600MPa, a metallographic structure of ferrite + pearlite, and uniform and fine grains.
[0008] The technical solution adopted by the present invention is:
[0009] A method for producing a hot-rolled wire rod for low-carbon alloy steel fiber, characterized in that the chemical composition of the hot-rolled wire rod includes, by mass percentage: C: 0.18-0.23%, Si≤0.10%, Mn: 0.50-0.80%, P≤0.015%, S≤0.010%, Cr: 0.015-0.30%, Ti: 0.03-0.05%, B: 0.0015-0.0040%, Al≥0.02%, and the rest is Fe and unavoidable impurities; the specification of the hot-rolled wire rod is Φ5.5mm.
[0010] Furthermore, the key production process of the hot-rolled wire rod includes continuous casting, rolling, spinning and cooling, and the specific steps are:
[0011] (1) In the continuous casting process: an integral nozzle tundish is used, the mold protection slag is medium carbon steel protection slag, the superheat is controlled at 25-30°C, the casting speed is controlled at 2.3-2.7 m / min, and the specific water volume is 0.8 L / kg;
[0012] (2) In the rolling process: low temperature rolling is adopted, and the temperature of the finishing mill is 800-840°C;
[0013] (3) In the spinning process: after rolling, the spinning is carried out at a low temperature, and the spinning temperature is 760-790°C;
[0014] (4) During the cooling process: cool down the Stelmo controlled cooling line, close the 1st to 5th Stelmo insulation covers and cool to 650-680°C at a cooling rate of 1-1.5°C / s, open the 6th to 8th insulation covers and cool to 550-580°C at a cooling rate of 2-2.5°C / s, and close all insulation covers after the 8th section.
[0015] Preferably, the chemical composition of the hot-rolled wire rod includes, by mass percentage: C: 0.19%, Si: 0.07%, Mn: 0.85%, P: 0.012%, S: 0.001%, Cr: 0.25%, Ti: 0.04%, B: 0.0021%, Al: 0.0027%, and the rest is Fe and unavoidable impurities.
[0016] Preferably, the chemical composition of the hot-rolled wire rod includes, by mass percentage: C: 0.19%, Si: 0.08%, Mn: 0.83%, P: 0.011%, S: 0.0009%, Cr: 0.25%, Ti: 0.04%, B: 0.0023%, Al: 0.0025%, and the rest is Fe and unavoidable impurities.
[0017] Further preferably, in the hot rolled wire rod continuous casting process, the superheat is controlled at 25-29°C, and the pulling speed is controlled at 2.5-2.7 m / min; in the rolling process, the temperature of the finishing mill is 810-830°C; the spinning temperature is 770-780°C, and in the cooling process, the Stelmor 1st-5th section insulation covers are closed and cooled to 650-680°C at a cooling rate of 1.2°C / s, and the 6th-8th section insulation covers are opened and cooled to 550-580°C at a cooling rate of 2.2°C / s.
[0018] Further preferably, in the hot rolled wire rod continuous casting process, the superheat is controlled at 26-29° C., and the drawing speed is controlled at 2.4-2.6 m / min.
[0019] Furthermore, the hot-rolled wire rod has a tensile strength of 550-600 MPa, a grain size of ≥9.0, and a structure of ferrite+pearlite.
[0020] The principle adopted by the method of the present invention is that adding Ti has a fine grain strengthening effect, adding B can improve the permeability of the wire rod, and can improve the strength under the same cooling conditions; however, adding too little B and Ti will not work, adding too much will be wasteful, and adding too much Ti inclusion content will have a great impact on the wire drawing, so the present invention selects a Ti content of 0.03-0.05% and a B content of 0.0015-0.0040%.
[0021] The beneficial effects of the present invention are:
[0022] (1) According to the user's requirements for hot-rolled wire rods for low-carbon alloy steel fibers and combined with the existing equipment capabilities, the steelmaking, rolling and cooling process research was carried out to produce wire rods with a hot-rolled tensile strength of 550-600MPa, a grain size ≥9.0, and a structure of ferrite + pearlite, which has broad application prospects and huge economic benefits.
[0023] (2) The present invention adds B and Ti through the design of reasonable chemical composition; the addition of Ti has a fine grain strengthening effect, and the addition of B can improve the permeability of the wire rod and can improve the strength under the same cooling conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0025] Figure 1 Metallographic structure diagram of wire rod according to Example 1 of the present invention;
[0026] Figure 2 Metallographic structure diagram of wire rod according to embodiment 2 of the present invention;
[0027] Figure 3 Metallographic structure diagram of the wire rod of comparative example 2 of the present invention. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Embodiment 1:
[0030] The invention discloses a production method of hot-rolled wire rod for low-carbon alloy steel fiber, with a rolling specification of Φ5.5mm.
[0031] The chemical composition by mass percentage includes: C: 0.19%, Si: 0.07%, Mn: 0.85%, P: 0.012%, S: 0.001%, Cr: 0.25%, Ti: 0.04%, B: 0.0021%, Al: 0.0027%, and the rest is Fe and unavoidable impurities. See Table 1 for details.
[0032] The key process steps are as follows:
[0033] In the continuous casting process: the continuous casting adopts an integral nozzle tundish, the mold protection slag adopts medium carbon steel protection slag, the superheat is controlled at 25-29°C, the casting speed is controlled at 2.5-2.7m / min, and the specific water volume is 0.8L / kg;
[0034] In the rolling process: the temperature of the finishing mill is controlled at 810-830℃;
[0035] In the spinning process: after rolling, the spinning is carried out at a low temperature, and the spinning temperature is 770-780℃;
[0036] In the cooling process: after rolling, it is cooled through the Stelmor controlled cooling line, the 1st to 5th Stelmor insulation covers are closed and cooled to 650-680°C at a cooling rate of 1.2°C / s, the 6th to 8th insulation covers are opened and cooled to 550-580°C at a cooling rate of 2.2°C / s, and all insulation covers after the 8th section are closed.
[0037] The metallographic structure of the Φ5.5mm hot-rolled wire rod obtained by the above method is ferrite + pearlite, and the grain size is grade 10. Figure 1 shown.
[0038] The tensile strength of hot-rolled wire rod is shown in Table 2.
[0039] Embodiment 2:
[0040] The invention discloses a production method of hot-rolled wire rod for low-carbon alloy steel fiber, with a rolling specification of Φ5.5mm.
[0041] The chemical composition by mass percentage includes: C: 0.19%, Si: 0.08%, Mn: 0.83%, P: 0.011%, S: 0.0009%, Cr: 0.25%, Ti: 0.04%, B: 0.0023%, Al: 0.0025%, and the rest is Fe and unavoidable impurities. See Table 1 for details.
[0042] The key process steps are as follows:
[0043] In the continuous casting process: the continuous casting adopts an integral nozzle tundish, the mold protection slag adopts medium carbon steel protection slag, the superheat is controlled at 26-29°C, the casting speed is controlled at 2.4-2.6m / min, and the specific water volume is 0.8L / kg;
[0044] In the rolling process: the temperature of the finishing mill is controlled at 810-830℃;
[0045] In the spinning process: after rolling, the spinning is carried out at a low temperature, and the spinning temperature is 770-780℃;
[0046] In the cooling process: after rolling, it is cooled through the Stelmor controlled cooling line, the 1st to 5th Stelmor insulation covers are closed and cooled to 650-680°C at a cooling rate of 1.2°C / s, the 6th to 8th insulation covers are opened and cooled to 550-580°C at a cooling rate of 2.2°C / s, and all insulation covers after the 8th section are closed.
[0047] The metallographic structure of the Φ5.5mm hot-rolled wire rod obtained by the above method is ferrite + pearlite, and the grain size is grade 10. Figure 2 shown.
[0048] The tensile strength of hot-rolled wire rod is shown in Table 2.
[0049] Comparative Example 1:
[0050] The invention discloses a production method of hot-rolled wire rod for low-carbon alloy steel fiber, with a rolling specification of Φ5.5mm.
[0051] The chemical composition by mass percentage includes: C: 0.20%, Si: 0.08%, Mn: 0.92%, P: 0.014%, S: 0.001%, Cr: 0.43%, Al: 0.0030%, and the rest is Fe and unavoidable impurities. See Table 1 for details.
[0052] The production steps different from Example 1 are:
[0053] In the rolling process: the temperature of the finishing mill is controlled at 880-900℃;
[0054] In the spinning process: after rolling, the spinning is carried out at a low temperature, and the spinning temperature is 850-870℃;
[0055] In the cooling process: after rolling, it is cooled through the Stelmor controlled cooling line, and the delayed cooling mode is used for slow cooling. The first three Stelmor insulation covers are opened, and the rest are all closed. The fans are all closed. The speed of the first section of the Stelmor roller is 0.2m / s, and each subsequent section increases by 0.05m / s.
[0056] The tensile strength of hot-rolled wire rod is shown in Table 2.
[0057] Comparative Example 2
[0058] The difference from Example 2 is that:
[0059] In the rolling process: the temperature of the finishing mill is controlled at 830-850℃;
[0060] In the spinning process: after rolling, the spinning is carried out at a low temperature, and the spinning temperature is 820-840℃;
[0061] In the cooling process: after rolling, it is cooled through the Stelmor controlled cooling line, and the fast cooling mode is adopted for fast cooling. The first 14 Stelmor insulation covers are opened, and the rest are all closed. The 1st to 7th fans are opened, and the fan air volume is 80%, and the other fans are all closed. The speed of the first section of the Stelmor roller is 0.6m / s, and each subsequent section increases by 0.05m / s.
[0062] The tensile strength of hot-rolled wire rod is shown in Table 2.
[0063] Table 1 Chemical composition content
[0064] chemical composition C% Si% Mn% P% S% Cr% Ti% B% Al% Example 1 0.19 0.07 0.85 0.012 0.001 0.25 0.04 0.0021 0.027 Example 2 0.19 0.08 0.83 0.011 0.0009 0.25 0.04 0.0023 0.025 Comparative Example 1 0.20 0.08 0.92 0.014 0.001 0.043 none none 0.030
[0065] Table 2 Hot rolled tensile strength of wire rod
[0066]
[0067] In summary, Cr can improve the strength of steel and has good hardenability; when steel contains trace amounts of B, the hardenability of steel can be doubled, which can improve the hot rolling performance of steel and increase strength; Ti can refine the grain structure of steel, thereby improving the strength and toughness of steel. Different cooling methods will result in different results. The hot-rolled tensile strength of the rapidly cooled wire rod is lower than the target requirement of ≥550MPa.
[0068] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.
Claims
1. A method for producing hot-rolled wire rod for low-carbon alloy steel fiber, characterized in that: The chemical composition of the hot-rolled wire rod includes, by mass percentage: C: 0.18-0.23%, Si≤0.10%, Mn: 0.50-0.80%, P≤0.015%, S≤0.010%, Cr: 0.015-0.30%, Ti: 0.03-0.05%, B: 0.0015-0.0040%, Al≥0.02%, and the rest is Fe and unavoidable impurities; the specification of the hot-rolled wire rod is Φ5.5mm.
2. The method for producing a hot-rolled wire rod for low-carbon alloy steel fiber according to claim 1, characterized in that: The key production process of the hot-rolled wire rod includes continuous casting, rolling, spinning and cooling, and the specific steps are as follows: (1) In the continuous casting process: an integral nozzle tundish is used, the mold protection slag is medium carbon steel protection slag, the superheat is controlled at 25-30°C, the casting speed is controlled at 2.3-2.7 m / min, and the specific water volume is 0.8 L / kg; (2) In the rolling process: low temperature rolling is adopted, and the temperature of the finishing mill is 800-840°C; (3) In the spinning process: after rolling, the spinning is carried out at a low temperature, and the spinning temperature is 760-790°C; (4) During the cooling process: cool down the Stelmo controlled cooling line, close the 1st to 5th Stelmo insulation covers and cool to 650-680°C at a cooling rate of 1-1.5°C / s, open the 6th to 8th insulation covers and cool to 550-580°C at a cooling rate of 2-2.5°C / s, and close all insulation covers after the 8th section.
3. The method for producing a hot-rolled wire rod for low-carbon alloy steel fiber according to claim 1, characterized in that: The chemical composition of the hot-rolled wire rod includes, by mass percentage, C: 0.19%, Si: 0.07%, Mn: 0.85%, P: 0.012%, S: 0.001%, Cr: 0.25%, Ti: 0.04%, B: 0.0021%, Al: 0.0027%, and the rest is Fe and unavoidable impurities.
4. The method for producing a hot-rolled wire rod for low-carbon alloy steel fiber according to claim 1, characterized in that: The chemical composition of the hot-rolled wire rod includes, by mass percentage, C: 0.19%, Si: 0.08%, Mn: 0.83%, P: 0.011%, S: 0.0009%, Cr: 0.25%, Ti: 0.04%, B: 0.0023%, Al: 0.0025%, and the rest is Fe and unavoidable impurities.
5. The method for producing a hot-rolled wire rod for low-carbon alloy steel fiber according to claim 3, characterized in that: In the hot-rolled wire rod continuous casting process, the superheat is controlled at 25-29°C, and the pulling speed is controlled at 2.5-2.7 m / min; in the rolling process, the temperature of the finishing mill is 810-830°C; the wire drawing temperature is 770-780°C, and in the cooling process, the Stelmor 1st-5th section insulation covers are closed and cooled to 650-680°C at a cooling rate of 1.2°C / s, and the 6th-8th section insulation covers are opened and cooled to 550-580°C at a cooling rate of 2.2°C / s.
6. The method for producing a hot-rolled wire rod for low-carbon alloy steel fiber according to claim 4, characterized in that: In the hot-rolled wire rod continuous casting process, the superheat is controlled at 26-29° C., and the drawing speed is controlled at 2.4-2.6 m / min.
7. The method for producing a hot-rolled wire rod for low-carbon alloy steel fiber according to any one of claims 1 to 6, characterized in that: The hot-rolled wire rod has a tensile strength of 550-600 MPa, a grain size of ≥9.0, and a structure of ferrite+pearlite.
Citation Information
Cited By
Production method of steel fiber wire rod
CN121496285A
A method for producing steel fibered wire rod