Low-cost 700MPa-grade axle housing steel and production method thereof

Through the C-Mn-Ti element system and optimized process steps, the problems of high carbon content, high cost and poor cold forming performance in high-strength axle steel are solved, and the production of low-cost 700MPa grade axle steel is achieved, satisfying the high-quality high-strength axle steel Requirements for strength and excellent cold forming performance.

CN119040762APending Publication Date: 2024-11-29武汉钢铁有限公司

Patent Information

Application Number
CN202411140698.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing high-strength axle shell steel with a level of above 600MPa has problems such as high carbon content, high production costs and poor cold forming performance, which cannot meet the lightweight needs of higher-end cars.

Method used

The C-Mn-Ti element system is adopted, combined with the solid solution strengthening of Mn element and the precipitation strengthening mechanism of effective Ti, and the production of low-cost 700MPa grade axle shell steel is achieved through the ultra-fast cooling fine crystal control of the temperature interval after the front cooling. . Specific processes include converter smelting, LHF treatment, continuous casting blanks, casting blank heating, rolling, cooling and coiling, and optimizing the chemical composition and process parameters of steel through deep desulfurization treatment, Ti alloy addition and laminar flow cooling.

Benefits of technology

While ensuring high-strength performance, excellent cold forming performance is obtained, the alloy cost is reduced, and the use needs of high-strength axle shell steel is met. The steel plate performance reaches yield strength ≥600MPa, tensile strength ≥700MPa, elongation ≥16% , the cold bending performance is qualified.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005000698640000051
    Figure BDA0005000698640000051
  • Figure BDA0005000698640000052
    Figure BDA0005000698640000052
  • Figure BDA0005000698640000061
    Figure BDA0005000698640000061
Patent Text Reader

Abstract

The invention discloses low-cost 700MPa-grade axle housing steel and a production method thereof. The low-cost 700MPa-grade axle housing steel comprises the following chemical components in percentage by weight: 0.03%-0.07% of C, 0.03%-0.50% of Si, 1.00%-1.20% of Mn, less than or equal to 0.015% of P, less than or equal to 0.005% of S, 0.015%-0.060% of Als, 0.10%-0.16% of Ti, less than or equal to 0.005% of N, 0.08%-0.14% of effective Ti and the balance of Fe and impurities. Wherein the effective Ti is equal to Ti <-3 >. 4N <-3 > S. The yield strength Rel of the 700MPa-grade axle housing steel is greater than or equal to 600MPa, the tensile strength Rm is greater than or equal to 700MPa, the elongation A is greater than or equal to 16%, the cold bending property D is equal to a, and the 700MPa-grade axle housing steel is qualified at 180 degrees. According to the invention, only a C-Mn-Ti element system is adopted, a dual strengthening mechanism combining solid solution strengthening of Mn element and precipitation strengthening of effective Ti is fully utilized, and fine grain control of a temperature interval after front-section cooling of ultra-fast cooling is carried out, so that the high-strength performance of the steel is ensured, meanwhile, excellent cold forming performance is achieved, and the use requirement of the high-strength axle housing steel is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of bridge shell steel processing, and in particular relates to high-strength bridge shell steel and a production method thereof. Background Art

[0002] Automobile axle housings have high safety requirements and need to meet strict component fatigue performance, which is reflected in the steel plates used for axle housings, which require stable performance, low temperature impact resistance, and good weldability. At present, the international standard for the strength of axle housing steel plates is up to Q460 level, and there is no higher grade technical standard.

[0003] CN104213019A discloses a 600MPa grade automobile bridge housing steel and a production method thereof, wherein the chemical composition thereof contains C 0.21% to 0.26%, Si 0.51% to 0.6%, Mn 1.1% to 1.5%, Al 0.01% to 0.06%, P≤0.02%, S≤0.01%, V 0.05% to 0.06%, N 0.012% to 0.016%, and the rest is Fe and unavoidable impurities, wherein V:N≤5:1. The method controls the contents of V and N elements while controlling rolling and cooling, and finally obtains a 600MPa grade hot-rolled strip steel for automobile bridge housing. In the design of the method: the C content is high, and the welding performance is poor; the V content is high, and the N element is difficult to control, and the production cost is high.

[0004] CN105239013A discloses a bridge housing steel for cold working and a manufacturing method thereof, wherein the chemical composition thereof contains C 0.08% to 0.18%, Si 0.10% to 0.45%, Mn 1.2% to 2.5%, Ti 0.01% to 0.05%, Al 0.02% to 0.35%, P ≤ 0.02%, S ≤ 0.010%, V 0.02% to 0.10%, Nb 0.015% to 0.10%, Cr 0.02% to 0.5%, and the rest is Fe and unavoidable impurities. The technology reduces the cost while ensuring the welding performance of the bridge housing steel for cold working, and finally obtains a 600MPa grade automobile bridge housing steel plate. Although the C and Si contents in the design of the method are not high, Cr and V alloys are also added, and the strength of the steel is only improved by the strengthening effect of the alloy elements, the production cost is high, and the yield strength of the steel does not exceed 600MPa.

[0005] CN111235460A discloses a bridge housing steel suitable for induction heating and a production method thereof, wherein the chemical composition contains, by mass percentage, C 0.15%-0.25%, Si 0.05%-0.18%, Mn 1.8%-3.0%, Ti 0.15%-0.30%, Al 0.02%-0.35%, P≤0.015%, S≤0.005%, N≤0.004%, and the rest is Fe and inevitable impurities. The yield strength of the bridge housing steel in hot-rolled state is ≥650MPa, the tensile strength is ≥750MPa, the elongation is ≥18%, and the impact energy at -20℃ is ≥150J; the yield strength of the bridge housing steel after induction heating is ≥520MPa, the tensile strength is ≥650MPa, the elongation is ≥25%, and the impact energy at -20℃ is ≥100J. In the design of this method: although the hot-rolled yield strength of the steel is ≥650MPa, the yield strength after heating is ≥520MPa, which is a significant decrease, and the C content is high, the welding performance is poor, the Mn and Ti contents are high, and the production cost is high.

[0006] CN114015934A discloses a 600MPa grade hot-rolled dual-phase structure bridge shell steel and a production method. The chemical composition contains C 0.06% to 0.10%, Si 0.05% to 0.20%, Mn 1.30% to 1.60%, P≤0.015%, S≤0.005%, Als 0.02% to 0.06%, and Nb 0.035% to 0.050% in terms of mass percentage. The design method of the invention adopts C-Mn-Nb component design strengthening. Although the carbon content is low and the welding performance is excellent, the yield strength can only be guaranteed to be above 500MPa. The coiling temperature range is difficult to control in the hot rolling process, the yield rate is low, and the production cost is high.

[0007] In summary, the existing high-strength bridge housing steels that reach the level of 600MPa and above have technical difficulties such as high carbon equivalent, high production cost, and poor cold forming performance, and cannot meet the needs of lightweighting of higher-end automobiles. Summary of the invention

[0008] The technical problem to be solved by the present invention is to provide a low-cost 700MPa-grade bridge shell steel and its production method in view of the deficiencies in the prior art, with yield strength Rel≥600MPa, tensile strength Rm≥700MPa, elongation A≥16%, and cold bending performance D=a, 180° qualified. The present invention only adopts the C-Mn-Ti element system, fully utilizes the dual strengthening mechanism combining the solid solution strengthening of the Mn element with the precipitation strengthening of effective Ti, and controls the fine grains in the temperature range after the ultra-fast cooling front section cooling, while ensuring the high strength performance of the steel, it has excellent cold forming performance, and meets the use requirements of high-strength bridge shell steel.

[0009] In order to solve the technical problem proposed by the present invention, the present invention provides a low-cost 700MPa grade bridge housing steel, the chemical composition and weight percentage content of which are: C 0.03% to 0.07%, Si 0.03% to 0.50%, Mn 1.00% to 1.20%, P≤0.015%, S≤0.005%, Als 0.015% to 0.060%, Ti 0.10% to 0.16%, N≤0.005%, and the rest are Fe and unavoidable impurities; wherein effective Ti is in the range of 0.08% to 0.14%, effective Ti=Ti-3.4N-3S, and is obtained according to the calculation formula of effective Ti according to the weight percentage of Ti, N and S, that is, w 有效(Ti) =w (Ti) -3.4w (N) -3w (S) .

[0010] Preferably, the weight percentage of C is 0.034-0.069%.

[0011] Preferably, the weight percentage of Si is between 0.032% and 0.461%.

[0012] Preferably, the weight percentage of Mn is 1.02-1.18%.

[0013] Preferably, the weight percentage content of Ti is 0.108-0.152%.

[0014] Preferably, the weight percentage of the effective Ti is between 0.082% and 0.137%.

[0015] The production method of the above-mentioned low-cost 700MPa grade bridge housing steel includes the following steps: converter smelting, LHF treatment, continuous casting, billet heating, rolling, cooling and coiling.

[0016] 1) After converter smelting, deep desulfurization treatment mode is adopted in LHF treatment, and the slag basicity is CaO / SiO2=2.0~3.0; after the first batch of desulfurized slag is added, the bottom blowing Ar gas volume is 70~90Nm 3 / h stirring for more than 3min; after the deep desulfurization treatment is completed and Ti alloy is added, the bottom blowing Ar gas volume is 10~30Nm 3 / h stirring for 5 minutes, and the total LHF treatment time is ≥18 minutes;

[0017] 2) After being cast into billets, the billets are heated: the billets are heated using a three-stage heating system, namely, the first heating stage, the second heating stage and the soaking stage, wherein the heating temperatures of the second heating stage and the soaking stage are controlled to be 1280-1320°C, the soaking time is ≥70min, and the total time in the furnace is ≥170min;

[0018] 3) Perform rough rolling and control the rough rolling outlet temperature at 1080-1120°C;

[0019] 4) Performing finishing rolling, controlling the starting temperature of finishing rolling to be between 1000 and 1100° C., and the final rolling temperature of finishing rolling to be between 860 and 910° C.;

[0020] 5) Cooling: During the cooling process, the steel is first cooled to 620°C to 660°C at a cooling rate of 25 to 40°C / s, and then laminar cooled to the coiling temperature;

[0021] 6) Coil the steel sheet and control the coiling temperature between 580 and 620 °C.

[0022] Functions and mechanisms of each element and main process in the present invention:

[0023] C: The C element has a solid solution strengthening effect. Low carbon steel can form needle-shaped or lath-shaped ferrite with excellent toughness during rolling and cooling, and can maintain good welding stability and reduce the risk of cracking. Taking all factors into consideration, the appropriate C content is 0.03-0.07%, preferably 0.034-0.069%.

[0024] Si: Si is a good deoxidizing element for molten steel. An appropriate amount of Si content is beneficial to reducing the loss of complete deoxidation of Al alloy and reducing steelmaking costs. Taking all factors into consideration, the appropriate Si content is 0.03-0.50%, preferably 0.032-0.461%.

[0025] Mn: Mn element forms manganese iron solid solution in steel, which can effectively improve the hardness and strength of steel. Considering the relationship between cost and performance, the appropriate Mn content is 1.0-1.2%, preferably 1.02-1.18%.

[0026] Al: Al is a necessary deoxidizing element for low alloy killed steel. The AlN element formed can effectively refine the grains. When the content is below 0.01%, deoxidation is insufficient. Taking all factors into consideration, the appropriate AlS content is 0.015-0.060%.

[0027] Ti: Ti can combine with N to form TiN during solidification, which is pinned to the grain boundary of austenite, hindering the growth of austenite grains and thus refining austenite grains. When Ti is dissolved in ferrite, its strengthening effect is higher than that of Al, Mn, Ni, Mo, etc. The effective Ti solid solution content (w 有效(Ti) =w (Ti) -3.4w (N) -3w (S)) is highly correlated with material strength. Taking all factors into consideration, the appropriate Ti content is 0.10-0.16%, preferably 0.108-0.152%; the appropriate effective Ti content is 0.08-0.14%, preferably 0.082-0.137%.

[0028] N: N is an inevitable residual element in steel. It can generate a small amount of nitrides such as SiN and AlN with Si and Al in steel, and can also play a role in refining grains. Taking all factors into consideration, N≤0.005%.

[0029] P, S: P in steel is easy to segregate and reduce the toughness and welding performance of steel. S is easy to form plastic sulfide and produce stratification defects. Therefore, the lower the P and S content, the better. Considering all factors, P≤0.015%, S≤0.005%.

[0030] The present invention adopts deep desulfurization treatment mode in LHF treatment, the slag basicity is CaO / SiO2=2.0-3.0; after the first batch of desulfurization slag is added, the bottom blowing Ar gas volume is 70-90Nm 3 / h stirring for more than 3min; after the deep desulfurization treatment is completed and Ti alloy is added, the bottom blowing Ar gas volume is 10~30Nm 3 / h stirring for 5 minutes, and the total LHF treatment time is ≥18 minutes. This is to reduce the oxidation of Ti element after the addition of Ti element and increase the solid solution content of effective Ti (w 有效(Ti) =w (Ti) -3.4w (N) -3w (S) ), reduce the number of Al2O3 inclusions and ensure the purity of steel.

[0031] The reason why the temperature of the second heating section and the final soaking section is controlled at 1280-1320°C, the heating and soaking time are not less than 70 minutes, and the total furnace time is controlled at not less than 170 minutes is that TiN generated by the combination of Ti and N can effectively inhibit the growth of austenite grains and ensure the refinement of the original austenite grains, and heating to 1280-1320°C can ensure that the Ti alloy element is completely dissolved and fully austenitized, effectively improving the strength performance of the steel.

[0032] The reason why the rough rolling outlet temperature is controlled at 1080-1120° C. in the present invention is to perform rough rolling in the recrystallization temperature zone.

[0033] The reason why the start temperature of finishing rolling is controlled at 1000-1100° C. and the final temperature of finishing rolling is controlled at 860-910° C. is to reduce the load of the rolling rolls and ensure uniform plastic deformation.

[0034] The reason why the present invention cools to 620°C to 660°C at a cooling rate of 25 to 40°C / s in the front stage and then cools to the coiling temperature in a laminar flow manner is to obtain a refined ferrite structure in the front stage of cooling and precipitate Ti elements in the laminar cooling and coiling stage to obtain the effect of grain strengthening.

[0035] The reason why the coiling temperature is controlled at 580-620° C. in the present invention is that the precipitation and solid solution strengthening effects of the Ti element can be fully exerted.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] 1) The present invention adopts the C-Mn-Ti element system, fully utilizes the dual strengthening mechanism of the solid solution strengthening of the Mn element and the precipitation fine grain strengthening of the effective Ti, and controls the fine grains in the temperature range after the ultra-fast cooling front section. While ensuring the high strength performance of the steel, it has excellent cold forming performance, and the alloy cost is low, meeting the use requirements of high-strength bridge shell steel. The steel plate performance is yield strength Rel ≥ 600MPa, tensile strength Rm ≥ 700MPa, elongation A ≥ 16%, and cold bending performance D = a, 180° qualified.

[0038] 2) The present invention innovatively improves the solid solution content of effective Ti and ensures the purity of steel by controlling the desulfurization mode, the selection of slag basicity, the timing of adding Ti alloy, the parameters and duration of bottom blowing Ar gas in the LHF treatment process, which is beneficial to improving the strength, plasticity and toughness of steel. The process is simple, the alloy cost is low, and improved production can be carried out under existing production conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is the metallographic structure diagram of the low-cost 700MPa grade cold-working bridge housing steel provided by the present invention. DETAILED DESCRIPTION

[0040] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the present invention is not limited to the following embodiments.

[0041] Embodiments 1 to 10 Each embodiment of the present invention produces low-cost 700 MPa grade bridge housing steel according to the following steps:

[0042] 1) After converter smelting, deep desulfurization treatment mode is adopted in LHF treatment, and the slag basicity is CaO / SiO2=2.0~3.0; after the first batch of desulfurized slag is added, the bottom blowing Ar gas volume is 70~90Nm 3 / h stirring for more than 3min; after the deep desulfurization treatment is completed and Ti alloy is added, the bottom blowing Ar gas volume is 10~30Nm 3 / h stirring for 5 minutes, and the total LHF treatment time is ≥18 minutes.

[0043] 2) After being cast into billets, the billets are heated: the billet heating adopts a three-stage heating system, namely the first heating stage, the second heating stage and the soaking stage. The heating temperature of the first heating stage is controlled to be 900-1100°C, and the heating time is ≥50min. The heating temperature of the second heating stage and the soaking stage is 1280-1320°C, and the soaking time is ≥70min. The total time in the furnace is ≥170min.

[0044] 3) Perform rough rolling and control the rough rolling outlet temperature at 1080-1120°C;

[0045] 4) Performing finishing rolling, controlling the starting temperature of finishing rolling to be between 1000 and 1100° C., and the final rolling temperature of finishing rolling to be between 860 and 910° C.;

[0046] 5) Cooling: During the cooling process, the steel is first cooled to 620°C to 660°C at a cooling rate of 25 to 40°C / s, and then laminar cooled to the coiling temperature;

[0047] 6) Coil the steel sheet and control the coiling temperature between 580 and 620 °C.

[0048] The comparative example was also produced by referring to the above steps, and the specific components and process parameters were carried out according to Table 1, Table 2 and Table 3.

[0049] Table 1 is a list of elemental composition values ​​of various embodiments and comparative examples of the present invention, and the rest are Fe and unavoidable impurities;

[0050] Table 2 shows the LHF process parameter values ​​of various embodiments of the present invention and comparative examples;

[0051] Table 3 shows the hot rolling process parameter values ​​of various embodiments of the present invention and comparative examples;

[0052] Table 4 is a list of performance test results of various embodiments of the present invention and comparative examples, wherein the yield strength (MPa), tensile strength (MPa), and elongation A are tested according to GB / T228 standard, and the cold bending performance is tested according to GB / T232 standard.

[0053] Table 1 List of chemical composition values ​​of various embodiments and comparative examples of the present invention (wt%)

[0054]

[0055] Note: *w 有效(Ti) =w (Ti) -3.4w (N) -3w (S) .

[0056] Table 2 LHF process parameter values ​​of various embodiments of the present invention and comparative examples

[0057]

[0058]

[0059] Table 3 Hot rolling process parameter values ​​of various embodiments of the present invention and comparative examples

[0060]

[0061] Table 4 Performance test results of various embodiments of the present invention and comparative examples

[0062]

[0063] As can be seen from Tables 1 and 4, the yield strength Rel≥600MPa, tensile strength Rm≥700MPa, elongation A≥16% of the bridge housing steel obtained in Examples 1 to 10, and the cold bending performance D=a, 180° are qualified. The component alloy cost in Comparative Example 1 is high, and the elongation is equivalent to that in the embodiment, but the yield strength and cold bending performance are lower than those in the embodiment; the steel carbon content in Comparative Example 2 is high, and the elongation is higher than that in the embodiment, but the yield strength and cold bending performance are lower than those in the embodiment. As can be seen from Tables 2 and 3, compared with the comparative example, the embodiment does not have a special and cumbersome production process, has strong applicability, does not require the investment of other process costs, and has a high yield rate.

[0064] The above embodiments are merely examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above descriptions. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived therefrom are still within the protection scope of the invention.

Claims

1. A low-cost 700MPa grade bridge housing steel, characterized in that: The chemical composition and weight percentage content are: C 0.03% ~ 0.07%, Si 0.03% ~ 0.50%, Mn 1.00% ~ 1.20%, P ≤ 0.015%, S ≤ 0.005%, Als 0.015% ~ 0.060%, Ti 0.10% ~ 0.16%, N ≤ 0.005%, and the rest are Fe and unavoidable impurities; among which, effective Ti = Ti-3.4N-3S, within the range of 0.08% ~ 0.14%.

2. The low-cost 700MPa grade bridge housing steel according to claim 1, characterized in that: The weight percentage of C is 0.034-0.069%.

3. The low-cost 700MPa grade bridge housing steel according to claim 1, characterized in that: The weight percentage of Si is 0.032-0.461%.

4. The low-cost 700MPa grade bridge housing steel according to claim 1, characterized in that: The weight percentage of Mn is 1.02-1.18%.

5. The low-cost 700MPa grade bridge housing steel according to claim 1, characterized in that: The weight percentage content of Ti is 0.108-0.152%.

6. The low-cost 700MPa grade bridge housing steel according to claim 1, characterized in that: The weight percentage of the effective Ti is 0.082-0.137%.

7. The method for producing low-cost 700MPa grade bridge housing steel according to claim 1, wherein the process comprises converter smelting, LHF treatment, continuous casting into billets, billet heating, rolling, cooling and coiling, characterized in that: 1) After converter smelting, deep desulfurization treatment mode is adopted in LHF treatment, and the slag basicity is CaO / SiO2=2.0~3.0; after the first batch of desulfurized slag is added, the bottom blowing Ar gas volume is 70~90Nm 3 / h stirring for more than 3min; after the deep desulfurization treatment is completed and Ti alloy is added, the bottom blowing Ar gas volume is 10~30Nm 3 / h stirring for 3 to 7 minutes, and the total LHF treatment time is ≥18 minutes; 2) After being cast into billets, the billets are heated: the billet heating adopts a three-stage heating system, namely the first heating stage, the second heating stage and the soaking stage, wherein the heating temperature of the second heating stage and the soaking stage is controlled to be 1280-1320°C, the soaking time is ≥70min, and the total time in the furnace is ≥170min; 3) Perform rough rolling and control the rough rolling outlet temperature at 1080-1120°C; 4) Performing finishing rolling, controlling the starting temperature of finishing rolling to be between 1000 and 1100° C., and the final rolling temperature of finishing rolling to be between 860 and 910° C.; 5) Cooling: During the cooling process, the steel is first cooled to 620°C to 660°C at a cooling rate of 25 to 40°C / s, and then laminar cooled to the coiling temperature; 6) Coil the steel sheet and control the coiling temperature between 580 and 620 °C.

8. The bridge shell steel produced by the method of claim 7, characterized in that: Yield strength Rel≥600MPa, tensile strength Rm≥700MPa, elongation A≥16%, cold bending performance D=a, 180° qualified.

Citation Information

Patent Citations

  • Steel for 10-ton axle shell and production method for steel

    CN102383035A

  • 780MPa grade high-fatigue high-strength steel and manufacturing method thereof

    CN109112422A

  • Low-temperature magnet yoke steel for large water-turbine generator set and production method

    CN115058660A

  • 700MPa-grade cold working forming axle housing steel with thickness of less than or equal to 10mm and production method of 700MPa-grade cold working forming axle housing steel

    CN116987970A

  • 700 mpa grade hot-formed axle housing steel and preparation method therefor

    WO2022063244A1

Cited By

  • Steel with yield strength of 700MPa for cold-formed high-fatigue axle housing and preparation method of steel

    CN120967245A