Heat treatment method for near-beta titanium alloy welding part

Through triple annealing treatment, the structural structure of the near-beta titanium alloy welded parts is regulated, forming dendritic flake structure, solving the problem of reduced joint strength and toughness after welding, significantly improving the comprehensive mechanical properties of the titanium alloy welded parts, and promoting the titanium alloy Engineering application of high-energy beam welding technology.

CN119040782APending Publication Date: 2024-11-29INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411393384.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-11-29

Smart Images

  • Figure CN119040782A_ABST
    Figure CN119040782A_ABST
Patent Text Reader

Abstract

The invention relates to a heat treatment method for a near-beta titanium alloy weldment, and the near-beta titanium alloy weldment is a weldment obtained by welding a first near-beta titanium alloy to-be-welded piece, a middle interlayer and a second near-beta titanium alloy to-be-welded piece together by adopting a high-energy beam welding process. The heat treatment method comprises the steps that a near-beta titanium alloy welding part is heated to a first temperature for first annealing treatment, and then cooling is conducted; the first temperature is 50-200 DEG C higher than the beta phase transformation point temperature of the near-beta titanium alloy welding part; the near-beta titanium alloy welding part obtained after first annealing treatment is heated to a second temperature for second annealing treatment, and then cooling is conducted; the second temperature is beta phase transformation point temperature + / -200 DEG C; the near-beta titanium alloy welding part obtained after second annealing treatment is heated to a third temperature for third annealing treatment, and the near-beta titanium alloy welding part obtained after heat treatment is obtained after cooling; and the third temperature is 50-500 DEG C lower than the beta phase transformation point temperature. The method is mainly used for improving the strength and toughness of the joint of the near-beta titanium alloy welding part.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of titanium alloys, in particular to a heat treatment method for a near-β titanium alloy welded piece. Background Art

[0002] Titanium alloys have the advantages of high strength, high heat resistance, and good corrosion resistance, and are widely used in important industrial fields such as aerospace, petrochemicals, and electronic power. Among them, near-β titanium alloys contain β stabilizing elements near the critical concentration, and the β phase stability coefficient K β =1.0~1.4, the volume fraction of β phase in the stable state is 25~50%. This type of alloy includes Ti-B19, TC17, TC18, TC21, etc., which have high strength and high toughness and have received extensive attention, especially in the development of large-scale engineering equipment such as aerospace aircraft fuselage structural parts, large ships and deep-sea detectors, and has broad application prospects. With the widespread application of near-β titanium alloys in large structural parts, its welding problems need to be solved urgently.

[0003] High-energy beam welding has the advantages of high energy density, strong penetration ability and high efficiency, and is widely used in the welding of near-β titanium alloy structural parts. However, during the high-energy beam welding process of near-β titanium alloy, the metastable β phase formed in the weld zone of the joint is relatively coarse, and the strengthening phase precipitated inside the β phase is very small, which seriously reduces the strength of the high-energy beam welded joint, making the tensile strength of the joint only about 70% of the parent material.

[0004] At present, in view of the problem of reduced joint mechanical properties of near-β titanium alloy after high-energy beam welding, related research mainly uses process parameter optimization and post-weld heat treatment to improve the performance of the joint. By optimizing process parameters such as strain rate, welding speed and scanning waveform, the grains are refined to a certain extent and the strength of the joint is slightly improved. Although the strength of the joint can be improved to a certain extent through the above welding process optimization, the improvement effect is not significant, only reaching about 80% of the strength of the parent material. In order to further improve the mechanical properties of the joint, heat treatment is usually used after welding to regulate the morphology and distribution of the strengthening phase, thereby improving the mechanical properties of the joint. After heat treatment, the strength of the joint has been improved to a certain extent, and the strength can reach more than 80% of the parent material, but the toughness has not been significantly improved. Therefore, obtaining a near-β titanium alloy joint with good strength and toughness matching has always been a difficult problem to solve.

[0005] In order to solve the problem of reduced strength of the joint of near-β titanium alloy after high-energy beam welding. The previous technology of the inventor of the present invention (application number 202311625514.1) proposes a welding method of near-β titanium alloy and a welded part of near-β titanium alloy, which mainly discloses: "Adding an intermediate interlayer between the parts to be welded of two near-β titanium alloy parts; wherein the material of the intermediate interlayer is an α-type or α+β-type titanium alloy with a volume fraction of β phase in the alloy not higher than 40% at room temperature; then, the two near-β titanium alloy parts to be welded and the intermediate interlayer are welded together by a high-energy beam welding process." Finally, a large amount of needle-shaped α phase is precipitated in the β phase, which significantly improves the strength of the joint, but the toughness is reduced. In addition, due to the fluctuation of the molten pool during the welding process, the element distribution inside the weld is uneven, which in turn affects the performance of the overall joint. Therefore, in view of the above-mentioned previous technology, a heat treatment method for near-β titanium alloy welded parts is urgently needed to improve the strength and toughness of the joints of near-β titanium alloy welded parts. Summary of the invention

[0006] In view of this, the present invention provides a heat treatment method for a near-β titanium alloy weldment, the main purpose of which is to improve the strength and toughness of the joint of the near-β titanium alloy weldment.

[0007] In order to achieve the above object, the present invention mainly provides the following technical solutions:

[0008] On the one hand, an embodiment of the present invention provides a heat treatment method for a near-β titanium alloy weldment, wherein the near-β titanium alloy weldment is a weldment obtained by welding a first near-β titanium alloy weldment, an intermediate interlayer, and a second near-β titanium alloy weldment together using a high-energy beam welding process; the material of the intermediate interlayer is an α-type titanium alloy or an α+β-type titanium alloy with a β phase volume fraction of not more than 40% at room temperature; wherein the heat treatment method comprises:

[0009] First annealing treatment: heating the near-β titanium alloy welded piece to a first temperature for first annealing treatment, and then cooling it to obtain a near-β titanium alloy welded piece after the first annealing treatment; wherein the first temperature is 50 to 200° C. higher than the β phase transformation point temperature of the near-β titanium alloy welded piece;

[0010] Second annealing treatment: heating the near-β titanium alloy welded piece after the first annealing treatment to a second temperature for second annealing treatment, and then cooling the piece to obtain a near-β titanium alloy welded piece after the second annealing treatment; wherein the second temperature is the β phase transformation point temperature of the near-β titanium alloy welded piece ±200°C;

[0011] Third annealing treatment: heating the near-β titanium alloy weld after the second annealing treatment to a third temperature for a third annealing treatment, and then cooling to obtain a near-β titanium alloy weld after heat treatment; wherein the third temperature is 50 to 500°C lower than the β phase transformation point temperature of the near-β titanium alloy weld.

[0012] Preferably, in the step of the first annealing treatment: the first temperature is 800-1100°C; and / or the time of the first annealing treatment is 1-4h; and / or after the first annealing treatment, the cooling rate is 0.2-100°C / s.

[0013] Preferably, in the near-β titanium alloy welded piece after the first annealing treatment: the weld zone is composed of lamellar primary α phase and interlaminar β phase; wherein the average thickness of the lamellar primary α phase is 0.3-1.2 μm.

[0014] Preferably, in the step of the second annealing treatment: the second temperature is 700-900°C; and / or the time of the second annealing treatment is 2-8h; and / or after the second annealing treatment, the cooling rate of the cold zone is 0.5-50°C / s.

[0015] Preferably, in the near-β titanium alloy welded piece after the second annealing treatment: the weld zone is composed of lamellar primary α phase and interlaminar β phase, wherein the average thickness of the lamellar primary α phase is 0.3-0.6 μm.

[0016] Preferably, in the step of the third annealing treatment: the third temperature is 400-700°C; and / or the time of the third annealing treatment is 2-10 hours; and / or after the third annealing treatment, the cooling rate is 0.5-50°C / s.

[0017] Preferably, in the near-β titanium alloy weld after heat treatment: the structure of the weld zone is a dendritic lamellar structure; wherein the dendritic lamellar structure includes lamellar primary α phase, interlaminar β phase and secondary α phase precipitated inside the interlaminar β phase; wherein the volume fraction of the lamellar primary α phase is greater than 50%, the volume fraction of the secondary α phase is greater than 3%, the average thickness of the lamellar primary α phase is 0.01 to 2 microns, and the average thickness of the secondary α phase is 0.01 to 0.3 microns.

[0018] Preferably, the thickness of the near-β titanium alloy weldment is greater than 10 mm.

[0019] Preferably, the step of welding the first near-β titanium alloy workpiece to be welded, the intermediate layer, and the second near-β titanium alloy workpiece to be welded together using a high-energy beam welding process comprises:

[0020] adding an intermediate layer between the to-be-welded portion of the first near-β titanium alloy to-be-welded part and the to-be-welded portion of the second near-β titanium alloy to-be-welded part to obtain an assembled part to be welded;

[0021] The first near-β titanium alloy to be welded part, the intermediate layer, and the second near-β titanium alloy to be welded part in the assembled parts to be welded are welded together by a high-energy beam welding process to obtain a near-β titanium alloy welded part;

[0022] Preferably, when the assembled parts to be welded are welded by a high-energy beam welding process, when the joint penetration reaches the thickness of the parts to be welded, and the intermediate interlayer and the welded parts of the two near-β titanium alloy parts to be welded are melted, and the weld is defect-free, the welding parameters of complete penetration at this time are determined as the process parameters during welding;

[0023] Preferably, when the high-energy beam welding process is an electron beam welding process, the welding parameters are controlled as follows: the electron beam scanning amplitude is 0.02 to 6 mm, the electron beam scanning frequency is 50 to 100 Hz, the acceleration voltage is 100 to 140 kV, the welding beam current is 40 to 90 mA, the welding speed is 300 to 800 mm / min, the focusing current is 2000 to 2400 mA, and the vacuum degree is 10 -5 ~10 -2 Pa.

[0024] On the other hand, an embodiment of the present invention provides a near-β titanium alloy weld after heat treatment, wherein the structure of the weld zone of the near-β titanium alloy weld after heat treatment is a dendritic lamellar structure; wherein the dendritic lamellar structure includes lamellar primary α phase, interlaminar β phase and secondary α phase precipitated inside the interlaminar β phase; wherein the volume fraction of the lamellar primary α phase is greater than 50%, the average thickness of the lamellar primary α phase is 0.01 to 2 microns, and the average thickness of the secondary α phase is 0.01 to 0.3 microns; preferably, the joint strength of the near-β titanium alloy weld after heat treatment is 800 to 1800 MPa, and the impact toughness is 10 to 100 J / cm2; preferably, the near-β titanium alloy weld after heat treatment is obtained by heat treating the near-β titanium alloy weld by the heat treatment method for a near-β titanium alloy weld described in any of the above items.

[0025] Compared with the prior art, the heat treatment method of a near-β titanium alloy weldment of the present invention has at least the following beneficial effects:

[0026] On the one hand, an embodiment of the present invention provides a heat treatment method for a near-β titanium alloy weldment, which is mainly a heat treatment method for the following near-β titanium alloy weldments:

[0027] The near-β titanium alloy weldment is a weldment obtained by welding together a first near-β titanium alloy weldment, an intermediate interlayer, and a second near-β titanium alloy weldment using a high-energy beam welding process; the material of the intermediate interlayer is an α-type titanium alloy or an α+β-type titanium alloy with a β phase volume fraction of no more than 40% at room temperature. Although the near-β titanium alloy weldment significantly improves the strength of the joint, its toughness is reduced. In addition, due to the fluctuation of the molten pool during the welding process, the elements inside the weld are unevenly distributed, which in turn affects the performance of the overall joint.

[0028] Here, in order to improve the strength and toughness of the joint of the above-mentioned near-β titanium alloy welded parts, the embodiment of the present invention proposes a heat treatment method, namely a triple annealing treatment (first annealing treatment, second annealing treatment, and third annealing treatment). Specifically, the chemical composition in the weld is uniformed by the first annealing treatment, so that the element distribution is more uniform, and a coarse lamellar structure is obtained; on the basis of the first annealing treatment, the coarse lamellar structure is further transformed by the second annealing treatment, which promotes more α phase nucleation and growth, and optimizes the lamellar structure; through the third annealing treatment, a finer secondary α phase is precipitated in the β phase, and finally a special dendritic lamellar structure (primary α phase + secondary α phase + β lamellar phase) is obtained, which enhances the α / β interface strengthening effect, thereby improving the comprehensive mechanical properties of the joint. Therefore, the solution of the embodiment of the present invention solves the problem that the strength and toughness of the joint of the near-β titanium alloy are reduced after high-energy beam welding.

[0029] In summary, the present invention provides a reference for the engineering application of high-energy beam welding of titanium alloys, greatly increases the application prospects of near-β titanium alloy welded joints, and promotes the industrial application of near-β titanium alloys.

[0030] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 Schematic diagram of the welding process of near-β titanium alloy welded parts; wherein (a) is a schematic diagram of the welding process without adding an intermediate interlayer; (b) is a schematic diagram of the welding process with adding a TC4 titanium alloy intermediate interlayer;

[0032] Figure 2 is a schematic diagram of a heat treatment method for a near-β titanium alloy weldment provided in an embodiment of the present invention;

[0033] Figure 3The macroscopic surface formation micrographs of the electron beam welded joint on the 30 mm thick near-β titanium alloy weldment; wherein (a) is a macroscopic surface formation micrograph of the welded joint without adding an intermediate interlayer; (b) is a macroscopic surface formation micrograph of the welded joint with adding a TC4 titanium alloy intermediate interlayer;

[0034] Figure 4 It is the microstructure morphology of the weld on the near-β titanium alloy weld after heat treatment; wherein, (a) is the microstructure morphology of the weld on the near-β titanium alloy weld without adding an intermediate interlayer; (b) is the microstructure morphology of the weld on the near-β titanium alloy weld with adding an intermediate interlayer;

[0035] Figure 5 The microstructure morphology of the weld on the near-β titanium alloy welded piece after annealing and heat treatment; wherein, (a) is the microstructure morphology of the weld after the first annealing treatment; (b) is the microstructure morphology of the weld after the second annealing treatment; (c) is the microstructure morphology of the weld after heat treatment;

[0036] Figure 6 It is the strength and toughness distribution diagram of the weld zone of the near-β titanium alloy weldment after heat treatment. DETAILED DESCRIPTION

[0037] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention application are described in detail below in conjunction with the accompanying drawings and preferred embodiments. In the following description, different "one embodiment" or "embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures, or characteristics in one or more embodiments may be combined in any suitable form.

[0038] Based on the problems existing in the high-energy beam welding joints of near-β titanium alloy weldments, the inventors of the present invention have conducted a lot of research and proposed in the previous technology (application number 202311625514.1): In the high-energy beam welding process of near-β titanium alloy parts, a titanium alloy (α-type titanium alloy or α+β-type titanium alloy, preferably TC4 titanium alloy) with excellent comprehensive performance and a volume fraction of β phase in the alloy of not more than 40% at room temperature is added between the welded parts to be welded, so as to hinder the direct combination of alloying elements in the near-β titanium alloy, and also balance the content of two-phase stabilizing elements, and promote the nucleation and growth of precipitation phases. Although the near-β titanium alloy weldment obtained by this technology improves the joint strength, the toughness is not improved. Therefore, it is necessary to heat treat it to improve the strength and toughness of the near-β titanium alloy weldment. However, the current heat treatment technology of titanium alloy weldments is not applicable to the above-mentioned near-β titanium alloy weldments. Therefore, for the above-mentioned near-β titanium alloy weldments, a matching heat treatment technology is urgently needed to improve the strength and toughness.

[0039] The present invention can even out the chemical composition in the weld by performing multiple annealing treatments on near-β titanium alloy welds, making the element distribution more uniform, and can also regulate the morphology and distribution of the α phase and the β phase, ultimately obtaining an excellent dendritic lamellar structure, thereby improving the comprehensive mechanical properties of the joint. The present invention is of great significance for promoting the engineering application of high-energy beam welding technology in the field of titanium alloy welding.

[0040] The specific scheme of the present invention is as follows:

[0041] An embodiment of the present invention provides a heat treatment method for a near-β titanium alloy weldment, wherein the near-β titanium alloy weldment is a weldment obtained by welding a first near-β titanium alloy weldment, an intermediate interlayer, and a second near-β titanium alloy weldment together using a high-energy beam welding process; the material of the intermediate interlayer is an α-type titanium alloy or an α+β-type titanium alloy having a β phase volume fraction of not more than 40% at room temperature; wherein the heat treatment method comprises:

[0042] First annealing treatment: heating the near-β titanium alloy weldment to a first temperature for first annealing treatment, and then cooling to obtain a near-β titanium alloy weldment after the first annealing treatment; wherein the first temperature is 50 to 200°C higher than the β phase transformation point of the near-β titanium alloy weldment. In this step, the first temperature is 800 to 1100°C, the holding time is 1 to 4 hours, and the cooling rate is 0.2 to 100°C / s.

[0043] Second annealing treatment: heating the near-β titanium alloy welded piece after the first annealing treatment to a second temperature for the second annealing treatment, and then cooling it to obtain the near-β titanium alloy welded piece after the second annealing treatment; wherein the second temperature is ±200°C of the β phase transformation point of the near-β titanium alloy welded piece. In this step, the second temperature is 700-900°C, the holding time is 2-8h, and the cooling rate is 0.5-50°C / s.

[0044] Third annealing treatment: heating the near-β titanium alloy welded piece after the second annealing treatment to a third temperature for the third annealing treatment, and then cooling it to obtain a near-β titanium alloy welded piece after heat treatment; wherein the third temperature is 50 to 500°C lower than the β phase transformation point of the near-β titanium alloy welded piece. In this step, the third temperature is 400 to 700°C, the holding time is 2 to 10 hours, and the cooling rate is 0.5 to 50°C / s.

[0045] The following explanations are required regarding the above scheme:

[0046] The heating temperature, holding time (annealing time) and cooling rate in the above heat treatment process can promote the phase transformation of more needle-shaped α phases in the near-β titanium alloy welded parts. The nucleation and growth of the α phase are promoted during the cooling process, and a large amount of lamellar structure is obtained. Too low heating temperature leads to less lamellar structure generated during the cooling process; too high heating temperature leads to serious oxidation of the weld surface, resulting in thicker oxide scale, which will reduce the surface quality of the weld. Moreover, the thick oxide scale attached to the surface will lead to uneven joint structure and performance during heat treatment. A uniform lamellar structure can be obtained when the annealing time is within the above range. Too short annealing time will lead to insufficient phase transformation and insufficient nucleation and growth of the lamellar structure; too long holding time will cause the generated lamellar structure to be severely coarsened, reducing the mechanical properties of the joint. A lamellar structure can be obtained when the cooling rate is within the above range. Too low cooling rate will make it difficult to obtain a stable lamellar structure; too high cooling rate will form martensite and other structures, and the generated martensite is fine, hard and brittle, which seriously reduces the toughness of the joint.

[0047] After electron beam welding of most near-β titanium alloy parts to be welded, the strength of the joints is reduced. However, after welding with the addition of α-type and α+β-type titanium alloy intermediate interlayers, the morphology and quantity of the precipitated phases are changed, and the strength of the joints is significantly improved, but the toughness is reduced. After the heat treatment of the present invention, a large amount of lamellar structure is precipitated in the joints, which significantly improves the strength and toughness of the joints. The technology of the present invention can even out the chemical composition in the weld, make the element distribution more uniform, and obtain excellent dendritic lamellar structure, providing a new method for the engineering application of titanium alloy electron beam welding.

[0048] In addition, the welding (butt welding) process of near-β titanium alloy weldments is described as follows:

[0049] First, an intermediate interlayer is added between the to-be-welded parts of two near-β titanium alloy parts to be welded to obtain an assembled part to be welded; wherein the material of the intermediate interlayer is an α-type or α+β-type titanium alloy in which the volume fraction of the β phase in the alloy is not higher than 40% at room temperature (that is, the near-β titanium alloy is subjected to high-energy beam welding by adding an α-type or α+β-type titanium alloy intermediate interlayer to achieve deep penetration welding of the near-β titanium alloy). Then, the two near-β titanium alloy parts and the intermediate interlayer in the assembled part to be welded are welded together by a high-energy beam welding process to obtain a near-β titanium alloy welded part.

[0050] For high-energy beam welding processes, there are mainly electron beam welding, laser beam welding, and plasma arc welding. Here, the present invention is mainly explained by taking electron beam welding as an example. Among them, during the electron beam welding process, the scanning amplitude of the electron beam is 0.02 to 6 mm. Here, the scanning amplitude of the electron beam is within this range mainly to ensure that during the electron beam scanning process, the energy transmission range is larger, the middle interlayer and the welded parts of the near-β titanium alloy to be welded on both sides are fully melted, and the alloy parts are tightly connected. However, if the amplitude is too small, it will lead to insufficient fusion, the interlayer is melted, and the welded parts of the near-β titanium alloy to be welded on both sides are not melted; if it is too large, it will cause the oscillation and disturbance of the molten pool to increase, resulting in poor weld formation. Among them, the thickness of the two near-β titanium alloy to be welded is greater than 10 mm. Among them, the selected thickness is within this range, that is, the near-β titanium alloy to be welded of medium and thick plates, during the electron beam welding process, due to the thickness of the plate, the precipitated phase in the weld has no time to grow and the number is small. The problem is more prominent, and the precipitated phase will also appear in the weld. The phenomenon of uneven distribution along the depth of penetration. The present invention can achieve the deep penetration welding of the near-β titanium alloy with an added intermediate interlayer, and can also achieve the homogenization of the weld structure. For a plate thickness less than this range, a lower heat input is required to achieve deep penetration welding, resulting in an increase in the number of precipitated phases and a relatively uniform distribution. Among them, in the electron beam welding process, the welding beam current is 40 to 90 mA, and the welding speed is 300 to 800 mm / min. Here, the welding beam current can achieve deep penetration welding of near-β titanium alloys within this range, and the joint is well formed and there are no welding defects on the surface. There is a certain matching relationship between the welding beam and the welding speed. Too low welding beam and welding speed will cause welding defects such as incomplete penetration and incomplete fusion; while too high welding beam and welding speed will cause cutting of the plate surface, poor weld surface forming, wider weld, and reduced joint mechanical properties. Among them, a large number of fine needle-shaped α phases are precipitated in the weld area of ​​the electron beam welded joint, and its volume fraction exceeds 50%, thereby improving the strength of the joint, but the toughness of the joint is reduced. In order to further improve the comprehensive mechanical properties of the joint of the near-β titanium alloy welded parts, the present invention performs multiple annealing treatments on the welded parts, which can even out the chemical composition in the weld, make the element distribution more uniform, and finally obtain a lamellar structure, thereby improving the comprehensive mechanical properties of the joint.

[0051] In addition, the design mechanism of the above-mentioned scheme of the present invention is as follows:

[0052] The invention solves the problem that less precipitated phase is produced in a near-β titanium alloy joint by the existing high-energy beam (eg electron beam) welding technology, and the mechanical properties of the joint are significantly reduced.

[0053] First, for electron beam welding of near-β titanium alloy parts, a coarse metastable β phase is first formed during the cooling process, and as the cooling process continues, a solid phase transformation occurs in the β phase. However, due to the very fast cooling rate during welding and the small proportion of α-phase stabilizing elements, it is difficult to precipitate the α phase. Therefore, only a small amount of needle-shaped α phase is generated inside the weld, which reduces the strength and toughness of the joint. Here, the present invention increases the content of α-phase stabilizing elements in the molten pool by adding an α-type or α+β-type titanium alloy with excellent comprehensive performance and a volume fraction of β phase in the alloy of not more than 40% at room temperature between two near-β titanium alloy parts, thereby balancing the proportion of two-phase stabilizing elements, promoting the nucleation and growth of the precipitated phase, and precipitating a large amount of needle-shaped α phase in the β phase, thereby improving the strength of the joint, but reducing the toughness. On this basis, in order to further improve the toughness of the joint, the present invention performs multiple annealing treatments on the welded parts to regulate the organization of the joint. Among them, the heating temperature of the first annealing treatment is usually higher than the β phase transformation point temperature, and it is kept warm for a certain time, and then the furnace is cooled to room temperature, so as to even out the chemical composition in the weld, make the element distribution more uniform, and obtain a coarse lamellar structure; the heating temperature of the second annealing treatment is ±200°C at the β phase transformation point of the weld, and it is kept warm for a certain time to make the coarse lamellar structure further undergo phase transformation, promote more α phase nucleation and growth, and optimize the lamellar structure; the heating temperature of the third annealing treatment is usually lower than the β phase transformation point temperature, and it is kept warm for a certain time to precipitate a finer secondary α phase in the β phase, and finally obtain a dendritic lamellar structure, enhance the α / β interface strengthening effect, and thus improve the comprehensive mechanical properties of the joint.

[0054] In addition, the present invention provides a reference for the engineering application of high-energy beam welding of titanium alloys, has the characteristics of high welding efficiency and high mechanical properties, and greatly increases the application prospects of near-β titanium alloy welded joints. Moreover, the improvement of welding performance can further promote the industrial application of near-β titanium alloys.

[0055] The present invention is further described below by specific embodiments:

[0056] Example 1

[0057] This embodiment mainly performs electron beam butt welding on two 30 mm thick near-β titanium alloy welded parts (plates, TC18 titanium alloy). After welding, the obtained near-β titanium alloy welded parts are heat treated. The main steps are as follows:

[0058] Cleaning steps: remove dust and oil from the surfaces, butt joints, and interlayers of two near-β titanium alloy welded parts (plates) (where the interlayer is α+β type TC4 titanium alloy with a thickness of 1 mm) to keep the butt joints and interlayers clean.

[0059] Assembly and welding steps: Place two near-β titanium alloy parts to be welded on a backing plate (where the backing plate is 10 mm thick and made of the same material as the near-β titanium alloy sheet to be welded). Add an intermediate layer between the two near-β titanium alloy parts to be welded to obtain the assembled parts to be welded. Subsequently, electron beam welding technology is used to butt weld the assembled parts to be welded to obtain a near-β titanium alloy welded part. The welding process is as follows: Figure 1 As shown in Figure (b) of the figure. The selected welding parameters are as follows: vacuum degree is 10 -4 Pa, acceleration voltage is 140 kV, welding speed is 300 mm / min, welding beam current is 75 mA, focusing current is 2292 mA, scanning frequency is 100 Hz, and scanning amplitude is 0.6 mm.

[0060] See also Figure 2 As shown, heat treatment of near-β titanium alloy weldments includes the following steps.

[0061] First annealing treatment: the near-β titanium alloy weld is placed in a high-temperature furnace, heated to 920°C (60°C higher than the β phase transformation point of the near-β titanium alloy weld) for the first annealing treatment (kept at 920°C for 2h), and then cooled (cooling rate of 0.5°C / s) to obtain the near-β titanium alloy weld after the first annealing treatment.

[0062] Second annealing treatment: The near-β titanium alloy weld after the first annealing treatment is heated to 700°C (160°C lower than the β phase transformation point of the near-β titanium alloy weld) for a second annealing treatment (kept at 700°C for 4 hours), and then cooled (cooling rate of 6°C / s) to obtain a near-β titanium alloy weld after the second annealing treatment.

[0063] Third annealing treatment: The near-β titanium alloy weld after the second annealing treatment is heated to 550°C (310°C lower than the β phase transformation point of the near-β titanium alloy weld) for the third annealing treatment (kept at the third annealing treatment temperature for 6 hours), and then cooled (cooling rate of 5°C / s) to obtain the near-β titanium alloy weld after heat treatment.

[0064] After triple annealing treatment, a finer secondary α phase is precipitated inside the β phase in this embodiment; a dendritic lamellar structure is formed in the weld zone, which is mainly composed of lamellar primary α phase, interlaminar β phase and secondary α phase, the volume fraction of the lamellar primary α phase is greater than 50%, the volume fraction of the secondary α phase is greater than 3%, the average thickness of the lamellar primary α phase is 0.01 to 2 microns, and the average thickness of the secondary α phase is 0.01 to 0.3 microns.

[0065] The mechanical properties of the heat-treated near-β titanium alloy welded parts obtained in this example are shown in Figure 6As shown, it can be seen that the tensile strength at the joint of the near-β titanium alloy welded piece after heat treatment in this embodiment is 986 MPa, and the impact toughness is 29 J / cm2.

[0066] Comparative Example 1

[0067] Comparative Example 1 mainly performs electron beam butt welding (without adding an intermediate interlayer) on two 30 mm thick near-β titanium alloy welded parts (plates, TC18 titanium alloy), and the main steps are as follows:

[0068] Cleaning steps: remove dust and oil from the surfaces and butt surfaces of the two near-β titanium alloy weldments to be welded, and keep the butt surfaces clean.

[0069] Assembly and welding steps: Place two near-β titanium alloy welded parts on a backing plate (wherein the backing plate is 10 mm thick and made of the same material as the near-β titanium alloy welded parts). No intermediate layer is added between the welded parts of the two near-β titanium alloy welded parts to obtain assembled welded parts. Subsequently, electron beam welding technology is used to butt weld the assembled welded parts. The welding process is as follows: Figure 1 As shown in Figure (a) in the figure. The selected welding parameters are as follows: vacuum degree is 10 -4 Pa, acceleration voltage is 140 kV, welding speed is 400 mm / min, welding beam current is 75 mA, focusing current is 2292 mA, scanning frequency is 100 Hz, and scanning amplitude is 0.6 mm.

[0070] Among them, the cross-sectional morphology and microstructure of the welded joint obtained in Comparative Example 1 are shown in Figure 3 Figure (a), Figure 4 As shown in Figure (a), it can be seen that electron beam welding achieves deep penetration welding of near-β titanium alloy, but under the same welding parameters, the weld width gradually decreases from the top to the root. Moreover, only a small amount of needle-shaped α phase precipitates in the weld area, and the volume fraction of α phase is less than 10%.

[0071] The mechanical properties of the joint obtained in Comparative Example 1 are shown in Figure 6 As shown, it can be seen that the tensile strength of the welded joint is only 845MPa, and the impact toughness is 8.9J / cm2, and the strength and toughness are relatively low.

[0072] Comparative Example 2

[0073] Comparative Example 2 mainly performs electron beam welding (adding an intermediate interlayer) on two 30 mm thick near-β titanium alloy welded parts (plates, TC18 titanium alloy), and the main steps are as follows:

[0074] Cleaning steps: remove dust and oil from the surfaces and butt surfaces of the two near-β titanium alloy weldments to be welded, and keep the butt surfaces clean.

[0075] Assembly and welding steps: Place two near-β titanium alloy parts to be welded on a backing plate (where the backing plate is 10 mm thick and made of the same material as the near-β titanium alloy sheet to be welded). Add a TC4 interlayer between the two near-β titanium alloy parts to be welded to obtain the assembled parts to be welded. Subsequently, the assembled parts to be welded are butt-welded using electron beam welding technology. The welding process is as follows: Figure 1 b. The selected welding parameters are as follows: vacuum degree is 10 -4 Pa, acceleration voltage is 140 kV, welding speed is 300 mm / min, welding beam current is 75 mA, focusing current is 2292 mA, scanning frequency is 100 Hz, and scanning amplitude is 0.6 mm.

[0076] Here, the cross-sectional morphology, microstructure, and mechanical properties of the welded parts of the near-β titanium alloy obtained in Example 2 are shown in FIG. Figure 3 Figure (b) and Figure 4 Figure (b) and Figure 6 As shown, it can be seen that electron beam welding is used to achieve deep penetration welding of near-β titanium alloy with an added TC4 titanium alloy intermediate layer, and the joint exhibits excellent parallel welds without welding defects; moreover, a large amount of needle-shaped α phase is precipitated in the weld zone on the joint, accounting for more than 50%, which greatly improves the strength of the joint, but reduces the toughness (the tensile strength of the joint is 960MPa, and the impact toughness is 7.6J / cm2).

[0077] Comparative Example 3

[0078] Comparative Example 3 mainly performs welding without adding an intermediate interlayer on two 30 mm thick near-β titanium alloy welded parts (plates, TC18 titanium alloy); after welding, the obtained near-β titanium alloy (TC18 titanium alloy) welded parts are subjected to double annealing treatment, and the main steps are as follows:

[0079] Cleaning steps: remove dust and oil from the surfaces and butt surfaces of the two near-β titanium alloy weldments to be welded, and keep the butt surfaces clean.

[0080] Assembly and welding steps: Place two near-β titanium alloy parts to be welded on a backing plate (wherein the backing plate is 10 mm thick and made of the same material as the near-β titanium alloy plate to be welded). No intermediate layer is added between the two parts to be welded to obtain the assembled parts to be welded. Subsequently, the assembled parts to be welded are butt-welded using electron beam welding technology. The welding process is as follows: Figure 1 As shown in Figure (a) in the figure. The selected welding parameters are as follows: vacuum degree is 10 -4Pa, acceleration voltage is 140 kV, welding speed is 400 mm / min, welding beam current is 75 mA, focusing current is 2292 mA, scanning frequency is 100 Hz, and scanning amplitude is 0.6 mm.

[0081] After welding, the obtained welded parts are subjected to double annealing treatment as follows:

[0082] First annealing treatment: The near-β titanium alloy welded part is placed in a high-temperature furnace, heated to 750°C (110°C lower than the β phase transformation point) for the first annealing treatment (kept at 750°C for 4 hours), and then cooled (cooling rate of 6°C / s) to obtain the near-β titanium alloy welded part after the first annealing treatment.

[0083] Second annealing treatment: The near-β titanium alloy weld after the second annealing treatment is heated to 580°C (280°C lower than the β phase transformation point) for a second annealing treatment (kept at the second annealing treatment temperature for 4 hours), and then cooled (cooling rate of 5°C / s) to obtain a near-β titanium alloy weld after heat treatment.

[0084] Among them, after welding and heat treatment of this comparative example, the volume fraction of α phase in the weld zone on the joint exceeds 50%, and the tensile strength of the joint is 1090MPa, but the toughness is not significantly improved, and the impact toughness is 14J / cm2.

[0085] Example 2

[0086] This embodiment mainly performs a first annealing treatment on the near-β titanium alloy (TC18 titanium alloy) weldment of Example 1, and studies the microstructure of the near-β titanium alloy weldment after the first annealing treatment. The main steps are as follows:

[0087] First annealing treatment: the near-β titanium alloy welded parts are placed in a high-temperature furnace for heating to a first temperature higher than the β phase transformation point temperature, kept at the first temperature for a certain period of time, and then cooled to room temperature. The selected heat treatment parameters are as follows: the heating temperature (first temperature) is 930°C, the holding time is 3h, and the cooling rate is 0.5°C / s.

[0088] Here, the microstructure of the weld zone on the near-β titanium alloy welded joint after the first annealing treatment is shown in Figure 5 As shown in Figure (a), it can be seen that the weld zone is mainly composed of relatively coarse lamellar primary α phase and interlaminar β phase, and the average thickness of the middle lamellar primary α phase is 0.3 to 1.2 μm (for thickness direction, see Figure 5 In the thickness direction as shown in Figure (a), the lamellar tissue is distributed relatively evenly.

[0089] Comparative Example 4

[0090] Comparative Example 4 mainly performs a first annealing treatment on the near-β titanium alloy (TC18 titanium alloy) weldment of Example 1, and combines Example 2 to study the influence of the temperature and time of the first annealing treatment on the microstructure of the near-β titanium alloy weldment after the first annealing treatment. The main steps are as follows:

[0091] The first annealing treatment: the near-β titanium alloy welded parts are placed in a high-temperature furnace for heating to a first temperature higher than the phase transition point, kept at the first temperature for a certain period of time, and then cooled to room temperature. The selected heat treatment parameters are as follows: the heating temperature (first temperature) is 1200°C, the holding time is 3h, and the cooling rate is 0.5°C / s.

[0092] The weld zone on the joint of the near-β titanium alloy welded piece after the first annealing treatment is mainly composed of coarse lamellar α phase and interlaminar β phase, and the average thickness of the α phase is 2.2-3 microns.

[0093] Here, the first annealing treatment selected in Comparative Example 4 uses too high a heating temperature, which causes the lamellar structure to be severely coarsened, affecting the performance of the joint. Moreover, too high a temperature can cause severe oxidation on the surface of the weld, generating a thick oxide scale, which can reduce the surface quality of the weld.

[0094] Example 3

[0095] This embodiment mainly performs a second annealing treatment on the near-β titanium alloy (TC18 titanium alloy) welded piece after the first annealing treatment obtained in Example 2, and studies the microstructure of the near-β titanium alloy welded piece after the second annealing treatment. The main steps are as follows:

[0096] Second annealing treatment: the near-β titanium alloy after the first annealing treatment is placed in a high-temperature furnace for heating to a temperature lower than the phase transition point or near the phase transition point (second temperature), kept at a certain temperature for a certain period of time, and then cooled to room temperature in air. The selected heat treatment parameters are as follows: the heating temperature (second temperature) is 750°C, the holding time is 5h, and the cooling rate is 6°C / s.

[0097] Among them, after welding in this embodiment, the microstructure of the weld zone on the near-β titanium alloy welded joint after the second annealing treatment is shown in Figure 5 As shown in Figure (b), it can be seen that the microstructure of the weld zone is mainly composed of optimized lamellar primary α phase and interlaminar β phase, and the average thickness of the lamellar primary α phase is 0.3 to 0.6 μm (for thickness direction, see Figure 5 In the thickness direction shown in (b) of FIG. 1 ). Here, the coarse lamellar structure undergoes further phase transformation during the second annealing treatment, promoting more α phase nucleation and growth, optimizing the lamellar structure, and making the weld area mainly composed of relatively fine lamellar structures, and the distribution of the lamellar structures is relatively uniform.

[0098] Comparative Example 5

[0099] Comparative Example 4 mainly performs a second annealing treatment on the near-β titanium alloy (TC18 titanium alloy) welded piece after the first annealing treatment obtained in Example 2, and combines Example 3 to study the effect of the second annealing treatment time on the microstructure of the near-β titanium alloy welded piece after the second annealing treatment. The main steps are as follows:

[0100] Second annealing treatment: The welded parts after the second annealing treatment are placed in a high temperature furnace for heating to the second temperature, kept at the temperature for a certain period of time, and then cooled to room temperature in air. The selected heat treatment parameters are as follows: the heating temperature (second temperature) is 750°C, the holding time is 9h, and the cooling rate is 6°C / s.

[0101] Here, although comparative example 5 also obtained a lamellar structure, the excessively long holding time caused the lamellar structure to be severely coarsened, and the lamellar thickness was even greater than the thickness of the lamellar structure after the first annealing treatment. In addition, being in a high temperature environment for a long time would also cause severe oxidation on the surface of the weld, thereby reducing the surface quality of the weld.

[0102] Example 4

[0103] This embodiment mainly performs a third annealing treatment on the near-β titanium alloy weldment (TC18 titanium alloy) obtained in Example 3 after the second annealing treatment, and the main steps are as follows:

[0104] Third annealing treatment: put the welded parts after the second annealing treatment into a high temperature furnace for heating, heating to a temperature lower than the phase change point (third temperature), keeping the temperature for a certain period of time, and then cooling to room temperature in the air to obtain the heat-treated parts. The selected heat treatment parameters are as follows: heating temperature (third temperature) is 580℃, holding time is 5h, and cooling rate is 5℃ / s.

[0105] The microstructure of the heat-treated near-β titanium alloy welded piece obtained in this embodiment is shown in Figure 5 As shown in Figure (c), it can be seen that after triple annealing, finer secondary α phase is precipitated inside the β phase; a dendritic lamellar structure is formed in the weld zone, which is mainly composed of lamellar primary α phase, interlaminar β phase and secondary α phase, the volume fraction of the lamellar primary α phase is greater than 50%, the volume fraction of the secondary α phase is greater than 3%, and the average thickness of the lamellar primary α phase is 0.01 to 2 microns (for thickness direction, see Figure 5 In the thickness direction shown in Figure (c), the average thickness of the secondary α phase is 0.01 to 0.3 microns.

[0106] See also Figure 5 As shown in Figure (c), it can be seen that compared with Comparative Example 1, the number of lamellar α phases precipitated at the joint weld of Example 4 is larger and densely distributed.

[0107] In addition, the tensile strength of the joint of the near-β titanium alloy welded part after heat treatment in this embodiment is 986 MPa, and the impact toughness is 29 J / cm2.

[0108] Comparative Example 6

[0109] Comparative Example 6 mainly performs a third annealing treatment on the near-β titanium alloy welded piece after the second annealing treatment obtained in Example 3, so as to study the influence of the third annealing treatment process parameters on the microstructure of the near-β titanium alloy welded piece after the heat treatment in combination with Example 4. The main steps are as follows:

[0110] Third annealing treatment: The near-β titanium alloy welded parts after the second annealing treatment are placed in a high-temperature furnace for heating. The heating temperature is usually lower than the phase transition point, and the temperature is kept for a certain period of time, and then cooled to room temperature in the air. Among them, the selected heat treatment parameters are as follows: heating temperature is 300℃, holding time is 5h, and cooling rate is 5℃ / s.

[0111] Here, since the heating temperature of the third annealing treatment in Comparative Example 6 is relatively low, a relatively fine secondary α phase is not precipitated inside the β phase. Moreover, due to the long-term heat preservation, the primary α phase further grows, which reduces the mechanical properties of the joint.

[0112] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A heat treatment method for near-β titanium alloy welded parts, It is characterized in that The near-β titanium alloy welded part is a welded part obtained by welding a first near-β titanium alloy welded part, an intermediate interlayer, and a second near-β titanium alloy welded part together by a high-energy beam welding process; the material of the intermediate interlayer is an α-type titanium alloy or an α+β-type titanium alloy with a β phase volume fraction of not more than 40% at room temperature; wherein the heat treatment method comprises: First annealing treatment: heating the near-β titanium alloy welded piece to a first temperature for first annealing treatment, and then cooling it to obtain a near-β titanium alloy welded piece after the first annealing treatment; wherein the first temperature is 50 to 200° C. higher than the β phase transformation point temperature of the near-β titanium alloy welded piece; Second annealing treatment: heating the near-β titanium alloy welded piece after the first annealing treatment to a second temperature for second annealing treatment, and then cooling the piece to obtain a near-β titanium alloy welded piece after the second annealing treatment; wherein the second temperature is the β phase transformation point temperature of the near-β titanium alloy welded piece ±200°C; Third annealing treatment: heating the near-β titanium alloy weld after the second annealing treatment to a third temperature for a third annealing treatment, and then cooling to obtain a near-β titanium alloy weld after heat treatment; wherein the third temperature is 50 to 500°C lower than the β phase transformation point temperature of the near-β titanium alloy weld.

2. The heat treatment method of the near-β titanium alloy weldment according to claim 1, It is characterized in that In the first annealing step: The first temperature is 800-1100° C.; and / or The first annealing treatment lasts for 1 to 4 hours; and / or After the first annealing treatment, cooling is performed at a cooling rate of 0.2 to 100° C. / s.

3. The heat treatment method of the near-β titanium alloy weldment according to claim 1 or 2, It is characterized in that In the near-β titanium alloy welded piece after the first annealing treatment: the weld zone is composed of lamellar primary α phase and interlaminar β phase; wherein the average thickness of the lamellar primary α phase is 0.3-1.2 microns.

4. The heat treatment method of a near-β titanium alloy weldment according to any one of claims 1 to 3, It is characterized in that In the step of the second annealing treatment: The second temperature is 700-900° C.; and / or The second annealing treatment time is 2 to 8 hours; and / or After the second annealing treatment, cooling is performed at a cooling rate of 0.5 to 50° C. / s.

5. The heat treatment method of a near-β titanium alloy weldment according to any one of claims 1 to 4, It is characterized in that In the near-β titanium alloy welded piece after the second annealing treatment: the weld zone is composed of lamellar primary α phase and interlaminar β phase, wherein the average thickness of the lamellar primary α phase is 0.3-0.6 micrometers.

6. A heat treatment method for a near-β titanium alloy weldment according to any one of claims 1 to 5, It is characterized in that In the step of the third annealing treatment: The third temperature is 400-700° C.; and / or The third annealing treatment lasts for 2 to 10 hours; and / or After the third annealing treatment, cooling is performed at a cooling rate of 0.5 to 50° C. / s.

7. A heat treatment method for a near-β titanium alloy weldment according to any one of claims 1 to 6, It is characterized in that In a near-β titanium alloy weld after heat treatment: the structure of the weld zone is a dendritic lamellar structure; wherein the dendritic lamellar structure includes a lamellar primary α phase, an interlaminar β phase, and a secondary α phase precipitated inside the interlaminar β phase; wherein the volume fraction of the lamellar primary α phase is greater than 50%, the volume fraction of the secondary α phase is greater than 3%, the average thickness of the lamellar primary α phase is 0.01 to 2 microns, and the average thickness of the secondary α phase is 0.01 to 0.3 microns.

8. The heat treatment method for a near-β titanium alloy weldment according to any one of claims 1 to 7, It is characterized in that The thickness of the near-β titanium alloy welded part is greater than 10 mm.

9. The heat treatment method for a near-β titanium alloy weldment according to any one of claims 1 to 8, It is characterized in that The step of welding the first near-β titanium alloy workpiece to be welded, the intermediate layer, and the second near-β titanium alloy workpiece to be welded together by using a high-energy beam welding process comprises: adding an intermediate layer between the to-be-welded portion of the first near-β titanium alloy to-be-welded part and the to-be-welded portion of the second near-β titanium alloy to-be-welded part to obtain an assembled part to be welded; The first near-β titanium alloy to be welded part, the intermediate layer, and the second near-β titanium alloy to be welded part in the assembled parts to be welded are welded together by a high-energy beam welding process to obtain a near-β titanium alloy welded part; Preferably, when the assembled parts to be welded are welded by a high-energy beam welding process, when the joint penetration reaches the thickness of the parts to be welded, and the intermediate interlayer and the welded parts of the two near-β titanium alloy parts to be welded are melted, and the weld is defect-free, the welding parameters of complete penetration at this time are determined as the process parameters during welding; Preferably, when the high-energy beam welding process is an electron beam welding process, the welding parameters are controlled as follows: the electron beam scanning amplitude is 0.02 to 6 mm, the electron beam scanning frequency is 50 to 100 Hz, the acceleration voltage is 100 to 140 kV, the welding beam current is 40 to 90 mA, the welding speed is 300 to 800 mm / min, the focusing current is 2000 to 2400 mA, and the vacuum degree is 10 -5 ~10 -2 Pa.

10. A heat-treated near-β titanium alloy weldment, It is characterized in that The microstructure of the weld zone of the near-β titanium alloy welded piece after the heat treatment is a dendritic lamellar microstructure; wherein the dendritic lamellar microstructure includes a lamellar primary α phase, an interlaminar β phase, and a secondary α phase precipitated inside the interlaminar β phase; wherein the volume fraction of the lamellar primary α phase is greater than 50%, the volume fraction of the secondary α phase is greater than 3%, the average thickness of the lamellar primary α phase is 0.01 to 2 microns, and the average thickness of the secondary α phase is 0.01 to 0.3 microns; Preferably, the joint strength of the near-β titanium alloy welded piece after heat treatment is 800-1800 MPa, and the impact toughness is 10-100 J / cm2; Preferably, the heat-treated near-β titanium alloy welded part is obtained by heat-treating the near-β titanium alloy welded part using the heat treatment method for a near-β titanium alloy welded part according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Near-beta titanium alloy welding method and near-beta titanium alloy welding part

    CN117381123A