System and method for electrochemically recovering phosphate positive electrode material
By using the electrochemical reaction between hypochlorite and phosphate cathode materials, lithium is recovered and phosphate precursors are regenerated, solving the problems of resource waste and high cost in lithium iron phosphate battery recycling, and realizing closed-loop recovery of lithium and high-value utilization of wastewater.
Patent Information
- Application Number
- CN202411342228.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-29
AI Technical Summary
In the current technology for recycling lithium iron phosphate batteries, byproducts cannot be effectively recovered, resulting in a large amount of wastewater and lithium loss, leading to high production costs and resource waste.
By reacting hypochlorite with phosphate-based cathode materials, lithium is recovered through an electrochemical method to generate lithium carbonate. The metal phosphate residue is regenerated into battery-grade phosphate precursors, and the wastewater is recycled by electrocatalytic reaction to generate hypochlorite, thus achieving closed-loop recovery of lithium and high-value recovery of wastewater.
It achieves closed-loop recovery of lithium, reduces production costs, improves lithium yield, and reduces wastewater discharge and resource waste through electrochemical recycling of leaching agents.
Smart Images

Figure CN119040922A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-ion batteries, and in particular to a system and method for electrochemically recovering phosphate positive electrode materials. Background Art
[0002] As new energy and environmental issues become increasingly prominent, the new energy vehicle and energy storage markets are experiencing explosive growth. Lithium iron phosphate (LFP) batteries occupy 70% of the new energy vehicle market due to their high energy density, long cycle life, and high safety and stability. Generally speaking, the service life of LFP batteries is 3-10 years, and the next few years will be the peak period for the retirement of LFP batteries. If a large number of discarded LFP batteries are not recycled, it will not only cause serious pollution to the environment, but also cause a waste of resources. The existing recycling of lithium iron phosphate cathode materials is only carried out by introducing hypochlorite for weak alkaline oxidation and selective leaching, but the following problems still exist: 1. During the wet recovery process, the by-products (such as chloride salts) produced cannot be effectively recovered and cannot be used at high value.
[0003] 2. The pH of the leaching solution in wet leaching is generally between 0 and 2. A large amount of wastewater and waste salt will be generated during the lithium precipitation process, increasing production costs.
[0004] 3. During the wet recovery process, a small amount of lithium will inevitably be entrained in the wastewater, and the loss of this lithium is inevitable. Summary of the invention In view of the above problems existing in the prior art, the object of the present invention is to provide a system and method for electrochemically recovering phosphate positive electrode materials, wherein a lithium-containing solution and a metal phosphate residue are obtained by reacting hypochlorite with a phosphate positive electrode material, the lithium-containing solution undergoes a carbonation reaction to obtain lithium carbonate and chlorine-containing wastewater, the metal phosphate residue undergoes a high-temperature solid-phase reaction to obtain a battery-grade phosphate precursor, and the lithium carbonate and the metal phosphate residue undergo a solid-phase reaction to regenerate battery-grade lithium iron phosphate, thereby realizing closed-loop recovery of lithium elements, and the generated chlorine-containing wastewater undergoes a bipolar membrane electrocatalytic process to generate new hypochlorite, which can be returned to the front end for recycling, thereby realizing high-value recovery of wastewater, realizing electrochemical recycling of leaching agents, and saving production costs.
[0005] The technical solution adopted by the present invention is to provide a system for electrochemically recovering phosphate positive electrode materials, comprising: A leaching kettle, used for receiving phosphate cathode waste and hypochlorite solution, and accommodating the phosphate cathode waste and hypochlorite solution to react; a first filter press, connected to the leaching kettle, receiving and separating the lithium-containing solution and the metal phosphate residue from the leaching kettle; A lithium precipitation kettle is connected to the first filter press, receives the lithium-containing solution separated from the first filter press, receives a lithium precipitation agent, and accommodates the lithium-containing solution and the lithium precipitation agent to react; The second filter press is connected to the lithium sinking kettle, and receives and separates the lithium carbonate and chlorine-containing wastewater from the lithium sinking kettle; A cleaning kettle is connected to the second filter press to receive and clean the lithium carbonate from the second filter press; A filtering and drying device, connected to the cleaning kettle, receives, filters and dries the lithium carbonate from the cleaning kettle; an evaporation and concentration device, connected to the second filter press, receiving and evaporating and concentrating the chlorine-containing wastewater from the second filter press; The electrochemical reactor is connected to the evaporation and concentration device, receives the chlorine-containing wastewater from the evaporation and concentration device, accommodates the chlorine-containing wastewater for electrochemical reaction, and circulates the hypochlorite solution obtained after the electrochemical reaction into the leaching kettle; The first push plate kiln is connected to the first filter press, receives the metal phosphate residue from the first filter press, and calcines the metal phosphate at high temperature; The second push plate kiln is connected to the first push plate kiln and the filtering and drying device, receives the battery-grade phosphate precursor from the first push plate kiln and the battery-grade lithium carbonate from the filtering and drying device, and accommodates the battery-grade phosphate precursor and the battery-grade lithium carbonate to react. Compared with the prior art, the technical effect achieved by the technical scheme is as follows: by using low-cost hypochlorite as an oxidant, the waste phosphate positive electrode waste is oxidized, the battery-grade iron phosphate and battery-grade carbonate are extracted, and finally the phosphate product can be regenerated by solid phase reaction, thereby realizing the closed-loop regeneration of the battery-grade phosphate product; there are lithium cations in the chlorine-containing wastewater, and the anions are chlorine elements. The chlorine-containing wastewater can generate new hypochlorite through electrocatalytic reaction, which can be returned to the leaching kettle for recycling, thereby realizing the high-value recovery of wastewater and the electrochemical recycling of the leaching agent. In addition, in the process of generating hypochlorite through multiple electrocatalytic reactions of the chlorine-containing wastewater in the bipolar membrane electrochemical reactor, a very small part of lithium is enriched in the hypochlorite each time, and is recovered to the leaching kettle with the hypochlorite. While the recovered hypochlorite reacts with a new batch of waste phosphate positive electrode waste, a very small part of lithium enriched in the hypochlorite also participates in the reaction again because the lithium concentration is increased by mixing with the waste phosphate positive electrode waste, thereby improving the total yield of the lithium element and realizing the closed-loop recovery of the lithium element.
[0006] In an optional embodiment, the filtering and drying device includes a third filter press and a disk dryer, the third filter press is connected to the cleaning kettle, receives and separates the lithium carbonate and the cleaning waste liquid after cleaning in the cleaning kettle, and the disk dryer is connected to the third filter press, receives and dries the lithium carbonate obtained from the third filter press.
[0007] Compared with the prior art, the technical effect achieved by adopting this technical solution is as follows: the setting of the third filter press enables the recycling of the cleaning waste liquid after solid-liquid separation of the third filter press, and the disc dryer is used to dry the lithium carbonate after passing through the third filter press to obtain battery-grade lithium carbonate.
[0008] In an optional embodiment, the system further comprises a reverse osmosis membrane, which is connected to the third filter press, receives and processes the cleaning waste liquid from the third filter press, and delivers the treated deionized water to the cleaning kettle via a pipeline.
[0009] Compared with the prior art, the technical effect achieved by adopting this technical solution is as follows: the reverse osmosis membrane is arranged so that the cleaning waste liquid after solid-liquid separation by the third filter press passes through the reverse osmosis membrane to provide deionized water for the cleaning kettle.
[0010] In an optional embodiment, the system also includes a batch mixer connected to the first push plate kiln and the disk dryer, receiving and mixing the phosphate precursor obtained from the first push plate kiln and the lithium carbonate obtained from the disk dryer, and sending the mixed material to the second push plate kiln through a pipeline.
[0011] Compared with the prior art, the technical effect achieved by adopting this technical solution is as follows: the batch mixer can stir and mix the battery-grade lithium carbonate and the battery-grade iron phosphate precursor, and then enter the second push-plate kiln for high-temperature calcination, so that the lithium carbonate and the iron phosphate precursor entering the second push-plate kiln can fully react to regenerate the battery-grade lithium iron phosphate positive electrode material.
[0012] In an optional embodiment, the electrochemical reactor is a bipolar membrane electrochemical reactor, which is a continuous flow pipe, a plurality of electrodes are embedded on the inner wall of the continuous flow pipe, a bipolar membrane is arranged in the middle of the continuous flow pipe, and the bipolar membrane isolates the bipolar membrane electrochemical reactor into a separate anode chamber and a cathode chamber.
[0013] Compared with the prior art, the technical effect achieved by adopting this technical solution is as follows: the electrochemical reactor is configured as a bipolar membrane, which can greatly reduce the internal resistance, and the bipolar membrane electrochemical reactor is configured as a continuous flow pipeline to realize continuous electrochemical reaction under high current density, and has excellent water dissociation performance and long-term use stability. The anode chamber of the bipolar membrane electrochemical reactor generates new hypochlorite in the chlorine-containing wastewater through an electrocatalytic reaction, and returns it to the front end for recycling, thereby realizing high-value recovery of wastewater, realizing electrochemical recycling of the leaching agent, and saving production costs.
[0014] In an optional embodiment, the cathode chamber is connected to the first pusher kiln through a pipeline, and the hydrogen obtained by the reaction in the cathode chamber enters the first pusher kiln through the pipeline as a reducing atmosphere. Compared with the prior art, the technical effect achieved by adopting this technical solution is that the cathode chamber of the bipolar membrane electrochemical reactor generates hydrogen through an electrocatalytic reaction, which is used as the reducing atmosphere of the first pusher kiln to generate battery-grade iron phosphate from ferrophosphorus residue, thereby realizing the recycling of hydrogen generated by the electrocatalytic reaction and saving production costs.
[0015] The present invention also provides a method for electrochemically recovering phosphate cathode materials, the method comprising the device as described in any of the above embodiments, comprising the following steps: S1: mixing the phosphate cathode waste with the hypochlorite solution in the leaching kettle, performing a weak alkalization reaction, and performing solid-liquid separation through the first filter press to obtain a lithium-containing solution and a metal phosphate residue; S2: subjecting the lithium-containing solution to a carbonation reaction in the lithium precipitation kettle, and performing solid-liquid separation through the second filter press to obtain lithium carbonate and chlorine-containing wastewater; S3: evaporating and concentrating the chlorine-containing wastewater in the evaporation and concentration device, entering the electrochemical reactor for electrocatalytic reaction to obtain a hypochlorite solution, and circulating the hypochlorite solution into the leaching kettle for reaction; S4: After the lithium carbonate is stirred and purified by the cleaning kettle, it is filtered and dried by the filtering and drying device to obtain battery-grade lithium carbonate; S5: calcining the metal phosphate residue in the first pusher kiln at high temperature to obtain a battery-grade phosphate precursor; S6: calcining the battery-grade lithium carbonate and the battery-grade phosphate precursor in the second pusher kiln at high temperature to generate a battery-grade phosphate positive electrode material.
[0016] Compared with the existing technology, the technical effect achieved by adopting this technical solution is as follows: by subjecting phosphate cathode waste to weak alkaline oxidation leaching, the purpose of preferential lithium extraction is achieved; the metal phosphate residue is refined into a battery-grade phosphate precursor through high-temperature roasting; the lithium salt is subjected to carbonation reaction to obtain battery-grade lithium carbonate; the lithium carbonate and phosphate precursor are subjected to solid-phase reaction to obtain battery-grade phosphate cathode material. The chlorine-containing wastewater generated after the lithium precipitation process produces new hypochlorite through electrocatalytic reaction, which can be returned to the front end for weak alkaline oxidation reaction, achieving the purpose of high value-added recycling of by-products.
[0017] In an optional embodiment, in S1, the phosphate cathode waste is mixed with the hypochlorite solution in a molar ratio of 1 to 5:1, and the solid-liquid ratio is 1 to 1000 g / L.
[0018] Compared with the prior art, the technical effect achieved by adopting this technical solution is that the phosphate cathode waste is mixed with the hypochlorite solution in a molar ratio of 1-5:1, and the solid-liquid ratio is 1-1000 g / L, so that the reaction in the leaching kettle is more complete.
[0019] In an optional embodiment, in S3, in S3, the chlorine-containing wastewater is evaporated and concentrated to 15-20 g / L in the evaporation concentration device.
[0020] Compared with the prior art, the technical effect achieved by adopting this technical solution is as follows: the chlorine-containing wastewater is evaporated and concentrated and then placed in the anode chamber for electrocatalytic reaction, thereby improving the recovery rate of hypochlorite and thus improving the single lithium yield.
[0021] In an optional embodiment, in S3, the working electrode of the electrocatalytic reaction is a graphite rod, the reference electrode is a mercuric oxide electrode, the electrolyte is a sodium chloride solution, and a step cyclic voltammetry electrochemical reaction is performed. The voltage range of the step cyclic voltammetry is 1.1-2.4V, the transition potential is 0.05V, and the current density is 10-20mA / cm 2 .
[0022] Compared with the prior art, the technical effect achieved by adopting the technical solution is as follows: the chlorine-containing wastewater is subjected to an electrocatalytic reaction, a step-by-step cyclic voltammetry electrochemical reaction is performed, and the recovery rate of hypochlorite is improved.
[0023] The beneficial effects of the embodiments of the present invention are as follows: a lithium-containing solution and a metal phosphate residue are obtained by reacting hypochlorite with phosphate cathode waste, the lithium-containing solution undergoes a carbonation reaction to obtain lithium carbonate and chlorine-containing wastewater, the metal phosphate residue undergoes a high-temperature solid-phase reaction to obtain a battery-grade phosphate precursor, and the lithium carbonate and the metal phosphate residue undergo a solid-phase reaction to regenerate a battery-grade phosphate product, thereby realizing closed-loop recovery of lithium elements, and the generated chlorine-containing wastewater undergoes a bipolar membrane electrocatalytic process to generate new hypochlorite, which can be returned to the front end for recycling, thereby realizing high-value recovery of wastewater, realizing electrochemical recycling of leaching agents, and saving production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 A schematic diagram of a system for electrochemically recovering phosphate cathode materials provided by an embodiment of the present invention is shown; Figure 2 A schematic diagram of a bipolar membrane electrochemical reactor according to an embodiment of the present invention is shown; Figure 3 A schematic flow chart of a method for electrochemically recovering phosphate cathode materials provided by an embodiment of the present invention is shown; Figure 4A schematic diagram of a method for electrochemically recovering phosphate positive electrode materials provided by an embodiment of the present invention is shown.
[0025] Description of reference numerals: 1- leaching kettle; 2- lithium precipitation kettle; 3- bipolar membrane electrochemical reactor; 31- anode chamber; 32- cathode chamber; 4- cleaning kettle; 5- first filter press; 6- second filter press; 7- third filter press; 8- first push plate kiln; 9- second push plate kiln; 10- reverse osmosis membrane; 11- disk dryer; 12- batch mixer; 13- evaporation concentration device. DETAILED DESCRIPTION
[0026] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention. It should be noted that relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements. See attached Figure 1 As shown, the present invention provides a system for electrochemically recovering phosphate positive electrode materials, comprising: A leaching kettle 1 is used to receive phosphate cathode waste and hypochlorite solution, and to accommodate the phosphate cathode waste and hypochlorite solution to react; A first filter press 5, connected to the leaching kettle 1, receives and separates the lithium-containing solution and the metal phosphate residue from the leaching kettle 1; The lithium precipitation kettle 2 is connected to the first filter press 5, receives the lithium-containing solution separated from the first filter press 5, receives the lithium precipitation agent, and accommodates the lithium-containing solution and the lithium precipitation agent to react; The second filter press 6 is connected to the lithium sinking kettle 2, and receives and separates the lithium carbonate and chlorine-containing wastewater from the lithium sinking kettle 2; The cleaning kettle 4 is connected to the second filter press 6 to receive and clean the lithium carbonate from the second filter press 6; A filtering and drying device, connected to the cleaning tank 4, receives, filters and dries the lithium carbonate from the cleaning tank 4; The evaporation and concentration device 13 is connected to the second filter press 6, and receives and evaporates and concentrates the chlorine-containing wastewater from the second filter press 6; The electrochemical reactor 3 is connected to the evaporation concentration device 13, receives the chlorine-containing wastewater from the evaporation concentration device 13, accommodates the chlorine-containing wastewater for electrochemical reaction, and circulates the hypochlorite solution obtained after the electrochemical reaction into the leaching kettle 1; The first push plate kiln 8 is connected to the first filter press 5, receives the metal phosphate residue from the first filter press 5, and calcines the metal phosphate at high temperature; The second pusher kiln 9 is connected to the first pusher kiln 8 and the filtering and drying device, receives the battery-grade phosphate precursor from the first pusher kiln 8 and the battery-grade lithium carbonate from the filtering and drying device, and accommodates the battery-grade phosphate precursor and the battery-grade lithium carbonate to react. Optionally, the phosphate cathode waste material may be lithium iron phosphate cathode waste material, and the hypochlorite solution may be a sodium hypochlorite solution.
[0027] Specifically, the lithium iron phosphate positive electrode waste and the sodium hypochlorite solution are mixed and reacted in the leaching kettle 1, and after the reaction, they enter the first filter press 5 for solid-liquid separation. The separated lithium-containing solution and residue (containing phosphorus slag, carbon, etc.), the residue enters the first push plate kiln 8 for high-temperature calcination to obtain a battery-grade iron phosphate precursor. The lithium-containing solution enters the lithium precipitation kettle 2 for lithium precipitation reaction, and is filtered by the second filter press 6 to obtain lithium carbonate and sodium chloride wastewater. The sodium chloride wastewater is passed through the electrochemical reactor 3 for electrocatalytic reaction to obtain a sodium hypochlorite solution, and the sodium hypochlorite solution is returned to the leaching kettle 1 for recycling. Lithium carbonate is stirred and purified by the cleaning kettle 4 to obtain battery-grade lithium carbonate, and the battery-grade lithium carbonate and the battery-grade iron phosphate precursor enter the second push plate kiln 9 for high-temperature calcination to obtain battery-grade lithium iron phosphate.
[0028] Specifically, metal cations such as lithium and sodium exist in the chlorine-containing wastewater, and the anion is chlorine. The wastewater can generate new hypochlorite through electrocatalytic reaction, which can be returned to the leaching kettle 1 for recycling, thereby realizing high-value recovery of wastewater and electrochemical recycling of the leaching agent. In addition, in the process of generating hypochlorite through multiple electrocatalytic reactions of the entire chlorine-containing wastewater in the electrochemical reactor 3, a very small amount of lithium is enriched each time, thereby improving the total yield of the lithium element and realizing closed-loop recovery of the lithium element.
[0029] See attached Figure 1As shown, in an optional embodiment, the filtering and drying device includes a third filter press 7 and a disk dryer 11, the third filter press 7 is connected to the cleaning kettle 4, receives and separates the lithium carbonate and the cleaning waste liquid after cleaning from the cleaning kettle 4, and the disk dryer 11 is connected to the third filter press 7, receives and dries the lithium carbonate obtained from the third filter press 7.
[0030] Specifically, the third filter press 7 is configured to allow the cleaning waste liquid after solid-liquid separation of the third filter press 7 to be recycled, and the disk dryer 11 is used to dry the lithium carbonate after passing through the third filter press 7 to obtain battery-grade lithium carbonate.
[0031] See attached Figure 1 As shown, in an optional embodiment, the system further includes a reverse osmosis membrane 10, which is connected to the third filter press 7, receives and processes the cleaning waste liquid from the third filter press 7, and delivers the treated deionized water to the cleaning kettle 4 through a pipeline.
[0032] Specifically, the reverse osmosis membrane 10 is arranged so that the cleaning waste liquid after solid-liquid separation by the third filter press 7 passes through the reverse osmosis membrane 10 to provide deionized water for the cleaning kettle 4 .
[0033] See attached Figure 1 As shown, in an optional embodiment, the system also includes a batch mixer 12, which is connected to the first push plate kiln 8 and the disk dryer 11, receives and mixes the phosphate precursor obtained from the first push plate kiln 8 and the lithium carbonate obtained from the disk dryer 11, and sends the mixed material to the second push plate kiln 9 through a pipeline.
[0034] Specifically, the batch mixer 12 can stir and mix the battery-grade lithium carbonate and the battery-grade iron phosphate precursor, and then enter the second pusher kiln 9 for high-temperature calcination, so that the lithium carbonate and the iron phosphate precursor entering the second pusher kiln 9 can fully react to regenerate the battery-grade lithium iron phosphate positive electrode material.
[0035] See attached Figure 2 As shown, in an optional embodiment, the electrochemical reactor 3 is a bipolar membrane electrochemical reactor, which is a continuous flow pipeline, a plurality of electrodes are embedded on the inner wall of the continuous flow pipeline, a bipolar membrane is arranged in the middle of the continuous flow pipeline, and the bipolar membrane isolates the bipolar membrane electrochemical reactor into a separate anode chamber 31 and cathode chamber 32.
[0036] Specifically, the electrochemical reactor 3 is configured as a bipolar membrane, which can significantly reduce the internal resistance, and the bipolar membrane electrochemical reactor is configured as a continuous flow pipeline. The continuous flow pipeline means that the liquid flows continuously in the pipeline, and the reactants are always in a flowing state. The continuous flow pipeline can realize continuous electrochemical reactions under high current density, and has excellent water dissociation performance and long-term use stability.
[0037] Specifically, an anode is arranged in the anode chamber 31 of the bipolar membrane electrochemical reactor, and the anode is a working electrode, and the working electrode is arranged as a graphite rod. A cathode is arranged in the cathode chamber 32, and the cathode is a reference electrode, and the reference electrode is arranged as a mercuric oxide electrode. Chlorine-containing wastewater enters the anode chamber 31, and generates a sodium hypochlorite solution after reaction, and deionized water enters the cathode chamber 32, and generates hydrogen after reaction.
[0038] See attached Figure 2 As shown, in an optional embodiment, the cathode chamber 32 is connected to the first pusher kiln 8 through a pipeline, and the hydrogen obtained by the reaction in the cathode chamber 32 enters the first pusher kiln 8 through the pipeline as a reducing atmosphere.
[0039] Specifically, the cathode chamber 32 of the bipolar membrane electrochemical reactor 3 generates hydrogen through an electrocatalytic reaction, and the hydrogen can be used as a reducing atmosphere of the first pusher kiln 8 to generate a battery-grade iron phosphate precursor from the residue, thereby realizing the recycling of hydrogen generated by the electrocatalytic reaction.
[0040] See attached Figure 3 and attached Figure 4 As shown, the present invention also provides a method for electrochemically recovering phosphate positive electrode materials.
[0041] The present invention also provides a method for electrochemically recovering phosphate cathode materials, the method comprising the device as described in any of the above embodiments, comprising the following steps: S1: mixing the phosphate cathode waste with the hypochlorite solution in a leaching kettle, performing a weak alkalization reaction, and performing solid-liquid separation through a first filter press to obtain a lithium-containing solution and a metal phosphate residue; S2: subjecting the lithium-containing solution to a carbonation reaction in a lithium precipitation kettle, and passing through a second filter press for solid-liquid separation to obtain lithium carbonate and chlorine-containing wastewater; S3: The chlorine-containing wastewater is evaporated and concentrated in an evaporation and concentration device, and enters an electrochemical reactor for electrocatalytic reaction to obtain a hypochlorite solution, and the hypochlorite solution is circulated into a leaching kettle for reaction; S4: After the lithium carbonate is purified by stirring in a cleaning kettle, it is filtered and dried to obtain battery-grade lithium carbonate after solid-liquid separation; S5: calcining the metal phosphate residue at high temperature in a first pusher kiln to obtain a battery-grade phosphate precursor; S6: The battery-grade lithium carbonate and the battery-grade phosphate precursor are subjected to high-temperature calcination in the second push-plate kiln to generate a battery-grade phosphate positive electrode material.
[0042] Specifically, the lithium carbonate in step S4 is purified by stirring in a cleaning kettle, and then passed through a third filter press for solid-liquid separation. The lithium carbonate obtained after solid-liquid separation enters a disk dryer for drying to obtain a battery-grade lithium carbonate product.
[0043] Specifically, in step S6, the battery-grade lithium carbonate and the battery-grade phosphate precursor enter the batch mixer for stirring and mixing, and then enter the second push plate kiln for high-temperature calcination to regenerate the battery-grade phosphate product.
[0044] Specifically, the purpose of preferential lithium extraction is achieved by subjecting phosphate cathode waste to weak alkaline oxidation leaching. The metal phosphate residue is refined into a battery-grade phosphate precursor through high-temperature roasting. The lithium salt undergoes a carbonation reaction to obtain battery-grade lithium carbonate. The lithium carbonate and the phosphate precursor undergo a solid-phase reaction to obtain a battery-grade phosphate cathode material. The chlorine-containing wastewater generated after the lithium precipitation process produces new hypochlorite through an electrocatalytic reaction, which can be returned to the front end for a weak alkaline oxidation reaction, achieving the purpose of recycling by-products with high added value.
[0045] In an optional embodiment, in S1, the phosphate cathode waste is mixed with the hypochlorite solution in a molar ratio of 1 to 5:1, and the solid-liquid ratio is 1 to 1000 g / L.
[0046] Specifically, the phosphate cathode waste and the hypochlorite solution can be mixed in a molar ratio of 2:1, and the solid-liquid ratio is 1000 g / L.
[0047] In an optional embodiment, in S3, the chlorine-containing wastewater is evaporated and concentrated to 15-20 g / L in an evaporation concentration device.
[0048] In an optional embodiment, in S3, the working electrode of the electrocatalytic reaction is a graphite rod, the reference electrode is a mercuric oxide electrode, the electrolyte is a sodium chloride solution, and a step cyclic voltammetry electrochemical reaction is performed. The voltage range of the step cyclic voltammetry is 1.1~2.4V, the transition potential is 0.05V, and the current density is 10~20mA / cm2.
[0049] Specifically, the electrolyte sodium chloride solution is chlorine-containing wastewater obtained by solid-liquid separation through a second filter press.
[0050] Example 1 This embodiment provides a method for electrochemically recovering phosphate positive electrode materials, the method comprising the following steps: S1: mixing the lithium iron phosphate positive electrode waste with the sodium hypochlorite solution in the leaching kettle at a molar ratio of 2:1, with a solid-liquid ratio of 1000 g / L, and performing a weak alkalization reaction for 3 hours, and performing solid-liquid separation through the first filter press to obtain a lithium-containing solution and an iron phosphate residue; S2: subjecting the lithium-containing solution to a carbonation reaction in the lithium precipitation kettle, and passing the second filter press to perform solid-liquid separation to obtain lithium carbonate and sodium chloride wastewater; S3: Evaporate and concentrate the sodium chloride wastewater to 20g / ml, and enter the bipolar membrane electrochemical reactor for electrocatalytic reaction to obtain a sodium hypochlorite solution, which can be circulated into the leaching kettle for reaction, wherein the working electrode of the electrocatalytic reaction is a graphite rod, the reference electrode is a mercuric oxide electrode, and the electrolyte is a sodium chloride solution. The electrochemical performance test of the step cyclic voltammetry method is carried out, and the voltage range of the step cyclic voltammetry method is 1.1~2.4V, the transition potential is 0.05V, and the current density is 10mA / cm 2 , the test time is 200s; S4: After the lithium carbonate is purified by stirring in a cleaning kettle, it is filtered and dried to obtain battery-grade lithium carbonate; S5: calcining the iron phosphate residue at high temperature in a first pusher kiln to obtain a battery-grade iron phosphate precursor; S6: Battery-grade lithium carbonate and battery-grade iron phosphate precursor are calcined at high temperature in a second pusher kiln to generate battery-grade lithium iron phosphate.
[0051] Example 2 This embodiment provides a method for electrochemically recovering phosphate positive electrode materials, the method comprising the following steps: S1: mixing the lithium iron phosphate positive electrode waste with the sodium hypochlorite solution in the leaching kettle at a molar ratio of 2:1, with a solid-liquid ratio of 1000 g / L, and performing a weak alkalization reaction for 3 hours, and performing solid-liquid separation through the first filter press to obtain a lithium-containing solution and an iron phosphate residue; S2: subjecting the lithium-containing solution to a carbonation reaction in the lithium precipitation kettle, and passing the second filter press to perform solid-liquid separation to obtain lithium carbonate and sodium chloride wastewater; S3: Evaporate and concentrate the sodium chloride wastewater to 15g / ml, and enter the bipolar membrane electrochemical reactor for electrocatalytic reaction to obtain a sodium hypochlorite solution, which can be circulated into the leaching kettle for reaction, wherein the working electrode of the electrocatalytic reaction is a graphite rod, the reference electrode is a mercuric oxide electrode, and the electrolyte is a sodium chloride solution. The electrochemical performance test of the step cyclic voltammetry method is carried out, and the voltage range of the step cyclic voltammetry method is 1.1~2.4V, the transition potential is 0.05V, and the current density is 12mA / cm 2 ,The test time is 200s; S4: After the lithium carbonate is purified by stirring in a cleaning kettle, it is filtered and dried to obtain battery-grade lithium carbonate; S5: calcining the iron phosphate residue at high temperature in a first pusher kiln to obtain a battery-grade iron phosphate precursor; S6: Battery-grade lithium carbonate and battery-grade iron phosphate precursor are calcined at high temperature in a second pusher kiln to generate battery-grade lithium iron phosphate.
[0052] Example 3 This embodiment provides a method for electrochemically recovering phosphate positive electrode materials, the method comprising the following steps: S1: mixing the lithium iron phosphate positive electrode waste with the sodium hypochlorite solution in the leaching kettle at a molar ratio of 2:1, with a solid-liquid ratio of 1000 g / L, and performing a weak alkalization reaction for 3 hours, and performing solid-liquid separation through the first filter press to obtain a lithium-containing solution and an iron phosphate residue; S2: subjecting the lithium-containing solution to a carbonation reaction in the lithium precipitation kettle, and passing the second filter press to perform solid-liquid separation to obtain lithium carbonate and sodium chloride wastewater; S3: Evaporate and concentrate the sodium chloride wastewater to 20g / ml, and enter the bipolar membrane electrochemical reactor for electrocatalytic reaction to obtain a sodium hypochlorite solution, which can be circulated into the leaching kettle for reaction, wherein the working electrode of the electrocatalytic reaction is a graphite rod, the reference electrode is a mercuric oxide electrode, and the electrolyte is a sodium chloride solution. The electrochemical performance test of the step cyclic voltammetry method is carried out, and the voltage range of the step cyclic voltammetry method is 1.1~2.4V, the transition potential is 0.05V, and the current density is 12mA / cm 2 ,The test time is 200s; S4: After the lithium carbonate is purified by stirring in a cleaning kettle, it is filtered and dried to obtain battery-grade lithium carbonate; S5: calcining the iron phosphate residue at high temperature in a first pusher kiln to obtain a battery-grade iron phosphate precursor; S6: Battery-grade lithium carbonate and battery-grade iron phosphate precursor are calcined at high temperature in a second pusher kiln to generate battery-grade lithium iron phosphate.
[0053] Example 4 This embodiment provides a method for electrochemically recovering phosphate positive electrode materials, the method comprising the following steps: S1: mixing the lithium iron phosphate positive electrode waste with the sodium hypochlorite solution in the leaching kettle at a molar ratio of 2:1, with a solid-liquid ratio of 1000 g / L, and performing a weak alkalization reaction for 3 hours, and performing solid-liquid separation through the first filter press to obtain a lithium-containing solution and an iron phosphate residue; S2: subjecting the lithium-containing solution to a carbonation reaction in the lithium precipitation kettle, and passing the second filter press to perform solid-liquid separation to obtain lithium carbonate and sodium chloride wastewater; S3: Evaporate and concentrate the sodium chloride wastewater to 20g / ml, and enter the bipolar membrane electrochemical reactor for electrocatalytic reaction to obtain a sodium hypochlorite solution, which can be circulated into the leaching kettle for reaction, wherein the working electrode of the electrocatalytic reaction is a graphite rod, the reference electrode is a mercuric oxide electrode, and the electrolyte is a sodium chloride solution. The electrochemical performance test of the step cyclic voltammetry method is carried out, and the voltage range of the step cyclic voltammetry method is 1.1~2.4V, the transition potential is 0.05V, and the current density is 20mA / cm 2 ,The test time is 200s; S4: After the lithium carbonate is purified by stirring in a cleaning kettle, it is filtered and dried to obtain battery-grade lithium carbonate; S5: calcining the iron phosphate residue at high temperature in a first pusher kiln to obtain a battery-grade iron phosphate precursor; S6: Battery-grade lithium carbonate and battery-grade iron phosphate precursor are calcined at high temperature in a second pusher kiln to generate battery-grade lithium iron phosphate.
[0054] Example 5 This embodiment provides a method for electrochemically recovering phosphate positive electrode materials, the method comprising the following steps: S1: mixing the lithium iron phosphate positive electrode waste with the sodium hypochlorite solution in the leaching kettle in a molar ratio of 2:1, with a solid-liquid ratio of 1 g / L, and performing a weak alkalization reaction for 3 hours, and performing solid-liquid separation through the first filter press to obtain a lithium-containing solution and an iron phosphate residue; S2: subjecting the lithium-containing solution to a carbonation reaction in the lithium precipitation kettle, and passing the second filter press to perform solid-liquid separation to obtain lithium carbonate and sodium chloride wastewater; S3: Evaporate and concentrate the sodium chloride wastewater to 20g / ml, and enter the bipolar membrane electrochemical reactor for electrocatalytic reaction to obtain a sodium hypochlorite solution, which can be circulated into the leaching kettle for reaction, wherein the working electrode of the electrocatalytic reaction is a graphite rod, the reference electrode is a mercuric oxide electrode, and the electrolyte is a sodium chloride solution. The electrochemical performance test of the step cyclic voltammetry method is carried out, and the voltage range of the step cyclic voltammetry method is 1.1~2.4V, the transition potential is 0.05V, and the current density is 10mA / cm 2 ,The test time is 200s; S4: After the lithium carbonate is purified by stirring in a cleaning kettle, it is filtered and dried to obtain battery-grade lithium carbonate; S5: calcining the iron phosphate residue at high temperature in a first pusher kiln to obtain a battery-grade iron phosphate precursor; S6: Battery-grade lithium carbonate and battery-grade iron phosphate precursor are calcined at high temperature in a second pusher kiln to generate battery-grade lithium iron phosphate.
[0055] Example 6 This embodiment provides a method for electrochemically recovering phosphate positive electrode materials, the method comprising the following steps: S1: mixing the lithium iron phosphate cathode waste with the sodium hypochlorite solution in the leaching kettle at a molar ratio of 4:1, with a solid-liquid ratio of 1000 g / L, and performing a weak alkalization reaction for 3 hours, and performing solid-liquid separation through the first filter press to obtain a lithium-containing solution and an iron phosphate residue; S2: subjecting the lithium-containing solution to a carbonation reaction in the lithium precipitation kettle, and passing the second filter press to perform solid-liquid separation to obtain lithium carbonate and sodium chloride wastewater; S3: Evaporate and concentrate the sodium chloride wastewater to 20g / ml, and enter the bipolar membrane electrochemical reactor for electrocatalytic reaction to obtain a sodium hypochlorite solution, which can be circulated into the leaching kettle for reaction, wherein the working electrode of the electrocatalytic reaction is a graphite rod, the reference electrode is a mercuric oxide electrode, and the electrolyte is a sodium chloride solution. The electrochemical performance test of the step cyclic voltammetry method is carried out, and the voltage range of the step cyclic voltammetry method is 1.1~2.4V, the transition potential is 0.05V, and the current density is 10mA / cm 2 ,The test time is 200s; S4: After the lithium carbonate is purified by stirring in a cleaning kettle, it is filtered and dried to obtain battery-grade lithium carbonate; S5: calcining the iron phosphate residue at high temperature in a first pusher kiln to obtain a battery-grade iron phosphate precursor; S6: Battery-grade lithium carbonate and battery-grade iron phosphate precursor are calcined at high temperature in a second pusher kiln to generate battery-grade lithium iron phosphate.
[0056] The sodium hypochlorite recovery rate and single lithium yield of the above examples were tested.
[0057] Specifically, the sodium hypochlorite recovery rate = (the amount of sodium hypochlorite produced / the amount of original sodium hypochlorite) × 100%; the single lithium recovery rate = (the amount of lithium recovered in a single time / the amount of lithium contained in the waste in a single time) × 100%.
[0058] The test results are shown in Table 1.
[0059] Table 1 From the analysis of Table 1, it can be seen that changing the concentration of sodium chloride wastewater to 15~20g / ml and the current density of step cyclic voltammetry to 10~20mA / cm 2 When the lithium iron phosphate cathode waste is mixed with the sodium hypochlorite solution in the leaching kettle in a molar ratio of 2:1, the solid-liquid ratio is 1000 g / L, the concentration of sodium chloride wastewater is 20 g / ml, and the current density of the step cyclic voltammetry is 10 mA / cm 2 When , the sodium hypochlorite recovery rate and single lithium yield are the highest.
[0060] Comparative Example 1 The difference between this comparative example and Example 1 is that the recycled raw material is ternary 811 positive electrode material, and the S3 electrocatalytic cycle process is not used.
[0061] The rest of the preparation methods and parameters were the same as those in Example 1.
[0062] Comparative Example 2 The difference between this comparative example and Example 1 is that the S3 electrocatalytic cycle process is not adopted.
[0063] The rest of the preparation methods and parameters were the same as those in Example 1.
[0064] The single lithium yield of the above comparative example was tested.
[0065] The test results are shown in Table 2.
[0066] Table 2 From the analysis of Table 2, it can be seen that the single lithium extraction efficiency of Comparative Example 1 is only 32.45%. The inventors analyzed that this may be because the recovery of ternary positive electrode materials generally adopts reducing reagents for recovery, while hypochlorite is oxidizing and is not suitable for the recovery of ternary positive electrode materials.
[0067] According to the comparative analysis of Table 1 and Table 2, the raw material recovered in Comparative Example 2 is phosphate positive electrode material, and the single lithium yield is relatively high. The recovery effect of Example 1 is the best. The generated chlorine-containing wastewater is subjected to a bipolar membrane electrocatalytic process to generate new hypochlorite, which can be returned to the front end for recycling, thereby achieving high-value recovery of wastewater, electrochemical recycling of leaching agents, and regeneration closed-loop recovery of lithium elements.
[0068] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A system for electrochemically recovering phosphate cathode materials, characterized in that: include: A leaching kettle (1) is used to receive phosphate cathode waste and hypochlorite solution, and to accommodate the phosphate cathode waste and hypochlorite solution to react; A first filter press (5) is connected to the leaching kettle (1) and receives and separates the lithium-containing solution and the metal phosphate residue from the leaching kettle (1); The lithium precipitation kettle (2) is connected to the first filter press (5), receives the lithium-containing solution separated from the first filter press (5), receives the lithium precipitation agent, and accommodates the lithium-containing solution and the lithium precipitation agent to react; The second filter press (6) is connected to the lithium precipitation kettle (2) and receives and separates the lithium carbonate and chlorine-containing wastewater from the lithium precipitation kettle (2); A cleaning kettle (4) is connected to the second filter press (6) to receive and clean the lithium carbonate from the second filter press (6); A filtering and drying device connected to the cleaning kettle (4) for receiving, filtering and drying the lithium carbonate from the cleaning kettle (4); an evaporation concentration device (13), connected to the second filter press (6), receiving and evaporating and concentrating the chlorine-containing wastewater from the second filter press (6); The electrochemical reactor (3) is connected to the evaporation concentration device (13), receives the chlorine-containing wastewater from the evaporation concentration device (13), accommodates the chlorine-containing wastewater for electrochemical reaction, and circulates the hypochlorite solution obtained after the electrochemical reaction into the leaching kettle (1); A first push plate kiln (8) is connected to the first filter press (5), receives the metal phosphate residue from the first filter press (5), and calcines the metal phosphate at a high temperature; The second push plate kiln (9) is connected to the first push plate kiln (8) and the filtering and drying device, receives the battery-grade phosphate precursor from the first push plate kiln (8) and the battery-grade lithium carbonate from the filtering and drying device, and accommodates the battery-grade phosphate precursor and the battery-grade lithium carbonate to react.
2. The system for electrochemically recovering phosphate cathode materials according to claim 1, characterized in that: The filtering and drying device comprises a third filter press (7) and a disk dryer (11); the third filter press (7) is connected to the cleaning kettle (4) to receive and separate the lithium carbonate and the cleaning waste liquid after cleaning in the cleaning kettle (4); and the disk dryer (11) is connected to the third filter press (7) to receive and dry the lithium carbonate obtained from the third filter press (7).
3. The system for electrochemically recovering phosphate cathode materials according to claim 2, characterized in that: It also includes a reverse osmosis membrane (10) which is connected to the third filter press (7), receives and processes the cleaning waste liquid from the third filter press (7), and delivers the deionized water obtained by the treatment to the cleaning kettle (4) through a pipeline.
4. The system for electrochemically recovering phosphate cathode materials according to claim 2, characterized in that: It also includes a batch mixer (12) connected to the first push plate kiln (8) and the disk dryer (11), receiving and mixing the phosphate precursor obtained from the first push plate kiln (8) and the lithium carbonate obtained from the disk dryer (11), and sending the mixed material to the second push plate kiln (9) through a pipeline.
5. The system for electrochemically recovering phosphate cathode materials according to claim 1, characterized in that: The electrochemical reactor (3) is a bipolar membrane electrochemical reactor, which is a continuous flow pipeline, a plurality of electrodes are embedded on the inner wall of the continuous flow pipeline, a bipolar membrane is arranged in the middle of the continuous flow pipeline, and the bipolar membrane isolates the bipolar membrane electrochemical reactor into a separate anode chamber (31) and cathode chamber (32).
6. The system for electrochemically recovering phosphate cathode materials according to claim 5, characterized in that: The cathode chamber (32) is connected to the first push plate kiln (8) via a pipeline, and the hydrogen obtained by the reaction in the cathode chamber (32) enters the first push plate kiln (8) through the pipeline as a reducing atmosphere.
7. A method for electrochemically recovering phosphate cathode materials, the method comprising the system according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1: mixing the phosphate cathode waste with the hypochlorite solution in the leaching kettle, performing a weak alkalization reaction, and performing solid-liquid separation through the first filter press to obtain a lithium-containing solution and a metal phosphate residue; S2: subjecting the lithium-containing solution to a carbonation reaction in the lithium precipitation kettle, and performing solid-liquid separation through the second filter press to obtain lithium carbonate and chlorine-containing wastewater; S3: evaporating and concentrating the chlorine-containing wastewater in the evaporation and concentration device, entering the electrochemical reactor for electrocatalytic reaction to obtain a hypochlorite solution, and circulating the hypochlorite solution into the leaching kettle for reaction; S4: After the lithium carbonate is stirred and washed in the cleaning kettle for purification, it is passed through the filtering and drying device for solid-liquid separation and drying to obtain battery-grade lithium carbonate; S5: calcining the metal phosphate residue in the first pusher kiln at high temperature to obtain a battery-grade phosphate precursor; S6: calcining the battery-grade lithium carbonate and the battery-grade phosphate precursor at high temperature in the second pusher kiln to generate a battery-grade phosphate positive electrode material.
8. The method for electrochemically recovering phosphate cathode materials according to claim 7, characterized in that: In S1, the phosphate cathode waste is mixed with the hypochlorite solution in a molar ratio of 1 to 5:1, and a solid-liquid ratio of 1 to 1000 g / L.
9. The method for electrochemically recovering phosphate cathode materials according to claim 7, characterized in that: In S3, the chlorine-containing wastewater is evaporated and concentrated to 15-20 g / L in the evaporation concentration device.
10. The method for electrochemically recovering phosphate cathode materials according to claim 7, characterized in that: In S3, the working electrode of the electrocatalytic reaction is a graphite rod, the reference electrode is a mercuric oxide electrode, the electrolyte is a sodium chloride solution, and a step cyclic voltammetry electrochemical reaction is performed. The voltage range of the step cyclic voltammetry is 1.1~2.4V, the transition potential is 0.05V, and the current density is 10~20mA / cm2.