Method for rapidly synthesizing large-current seawater electrolysis self-supporting corrosion-resistant anode catalyst at normal temperature and normal pressure

By electrodepositing on the current collector, the CoFe-LDH composite Ce(OH)3 heterostructure formed by forming a Cl-intercalation layer, the corrosion problem of Cl-to-anode catalyst in seawater is solved, and high activity and corrosion resistance are achieved. It is suitable for The electrolytic seawater hydrogen production technology has the prospect of industrial application.

CN119040945AActive Publication Date: 2024-11-29BEIJING INST OF TECH

Patent Information

Application Number
CN202411180638.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-29
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The high concentration of Cl- in seawater causes corrosion and activity to the anode catalyst during the hydrogen production process of electrolytic seawater. The use of metal nitrate raw materials during electrodeposition of existing CoFe-LDH catalysts leads to NO32-intercalation, which cannot effectively resist the corrosion of Cl-. Catalyst deactivation.

Method used

The CoFe-LDH composite Ce(OH)3 heterostructure with Cl-intercalated layer was formed on the current collector by electrodeposition method, and chlorine was added by using raw materials such as cobalt chloride hexahydrate, ferric nitrate nohydrate and cerium nitrate hexahydrate. Ammonium changes the electrolyte environment, forms a Cl-intercalation layer to resist Cl- in seawater, and performs electrodeposition at normal temperature and pressure to form a catalytic electrode without binder and conductive agent.

Benefits of technology

Achieves high activity and Cl-corrosion resistance to anode catalyst under high current electrolytic seawater conditions, reducing production costs, simplifying process flow, having industrial application prospects, and exhibiting excellent OER catalytic activity and stability in electrolytic seawater .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040945A_ABST
    Figure CN119040945A_ABST
Patent Text Reader

Abstract

The invention relates to a method for rapidly synthesizing a large-current seawater electrolysis self-supporting corrosion-resistant anode catalyst at normal temperature and normal pressure, which comprises the following steps: putting a current collector into an electrolyte containing cobalt chloride, ferric nitrate, cerous nitrate and ammonium chloride to carry out cathode electrodeposition; the Co < Fe >-LDH composite Ce (OH) 3 heterostructure catalytic electrode material of the Cl <-> intercalation electrodeposited on the current collector is obtained. The synthesis method provided by the invention is short in process, mild in condition and easy for large-scale production, and the heterostructure catalytic electrode material provided by the invention shows excellent catalytic activity and stability in an anode oxygen evolution reaction for hydrogen production by seawater electrolysis, and has potential commercial application prospects. The invention has great significance in promoting the development of green and clean energy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of preparation of electrochemical electrode materials, in particular to a Cl electrodeposited on a current collector. - An electrocatalyst for oxygen evolution reaction at the anode of high current electrolysis of seawater with an intercalated CoFe-LDH composite Ce(OH)3 heterostructure and a preparation method thereof. Background Art

[0002] The scarcity of fossil fuels and the increase in carbon dioxide emissions have accelerated the exploration of alternative energy sources. Hydrogen energy has a high specific energy density (142MJ kg -1 ) and non-polluting properties are considered to be ideal clean energy carriers. Water electrolysis hydrogen production technology has the advantages of non-polluting reaction process, can use waste heat or renewable intermittent energy (wind or solar energy) to generate electricity, and produces high purity hydrogen, making it a powerful means to achieve green hydrogen production. However, the huge global demand for hydrogen will undoubtedly aggravate the shortage of freshwater resources. Seawater accounts for about 96.5% of the total water resources. Using seawater instead of fresh water for electrolysis to produce hydrogen is a key technology that needs to be solved in the future development of hydrogen energy. However, the presence of Cl in seawater - Mg 2+ , Ca 2+ Impurities such as carbon dioxide and microorganisms make the electrolysis of seawater to produce hydrogen a major challenge.

[0003] Seawater electrolyzers consist of two half reactions: oxygen evolution reaction (OER) at the anode and hydrogen evolution reaction (HER) at the cathode. The challenges of hydrogen production by electrolyzing seawater mainly occur at the anode. - It will compete with OER at the anode to generate chlorine (chlorine evolution reaction, under acidic conditions) or hypochlorite (chlorine oxidation reaction, under alkaline conditions). OER is more likely to occur under alkaline conditions, and the theoretical voltage of OER under alkaline conditions is 490mV lower than that of chlorine oxidation reaction. Using a highly active catalyst to make the overpotential of OER lower than 490mV can avoid the occurrence of chlorine oxidation competition reaction and improve the anode OER selectivity. In addition, high concentrations of Cl - It will corrode the catalytic electrode material and cause the catalyst to deactivate quickly. - The corrosion catalytic material ensures that the catalytic electrode material can operate stably for a long time under high current electrolysis of alkaline seawater. The presence of Cl- seriously affects the activity and stability of the electrocatalytic material of the anode of seawater electrolysis. It is necessary to develop a catalyst with high OER activity and Cl-resistance. - Anode catalytic electrode materials for high-current seawater electrolysis that are corrosion-resistant and can be prepared on a large scale in a short time are key requirements for promoting the development of seawater electrolysis hydrogen production technology and realizing industrialization.

[0004] Layered double hydroxides (LDH) have been a hot topic in OER catalyst research in recent years, among which CoFe-LDH has shown great application potential due to its excellent anodic OER catalytic activity in water electrolysis. Electrodeposition is a preparation method that can quickly synthesize catalytic electrode materials at room temperature and pressure, and is easy to scale up for large-scale preparation. However, the CoFe-LDH currently prepared by electrodeposition mostly uses metal nitrates as raw materials, which makes it have NO3 2- When used as an anode catalyst for electrolysis of seawater, it will be rapidly corroded and deactivated because of the Cl - NO3 2- With stronger intercalation ability, Cl - Will continue to enter the CoFe-LDH interlayer to replace NO3 2- By replacing the high-cost cobalt nitrate raw material with low-cost cobalt chloride and adding a small amount of cheap ammonium chloride to change the electrolyte environment during deposition, a Cl - Intercalated CoFe-LDH, interlayer Cl - To Cl in seawater - The repulsive effect makes it stable for use in seawater electrolysis anode. In addition, OER is greatly affected by mass transfer behavior. Adding a small amount of cerium nitrate to the electrolyte during electrodeposition can obtain Cl - Intercalated CoFe-LDH composite Ce(OH)3 heterostructure electrocatalyst. Ce(OH)3 can be rapidly oxidized to CeO2 during the OER process. Based on the hard-soft acid-base theory, Ce 4+ It will preferentially adsorb OH in the electrolyte - , which not only further excludes Cl - , which promotes the mass transfer of OH- and accelerates the OER reaction kinetics. Summary of the invention

[0005] The present invention aims to provide a Cl in situ electrodeposited on a current collector. - Intercalated CoFe-LDH composite Ce(OH)3(CoFe-Cl - / Ce(OH)3) heterostructure catalyst, which can be directly used as a high-current electrolysis seawater anode OER catalytic electrode without the need for additional binders and conductive agents, and has good OER catalytic activity and high Cl resistance - The synthetic method has mild conditions, low cost, and is easy to scale up for production, and has excellent industrial application prospects.

[0006] To achieve this purpose, the present invention adopts the following technical solutions:

[0007] A method for rapidly synthesizing a self-supporting corrosion-resistant anode catalyst for large current electrolysis of seawater at room temperature and pressure, the specific steps are as follows: (1) Weighing cobalt chloride hexahydrate, ferric nitrate nonahydrate, cerium nitrate hexahydrate and ammonium chloride, adding them to deionized water, stirring them thoroughly to dissolve them completely to obtain an electrolyte solution for electrodeposition; (2) using a dual counter electrode-single working electrode electrodeposition system, connecting the current collector and the inert electrode plate to the cathode and anode of a DC power supply, respectively, and immersing them in the electrolyte solution obtained in step (1); (3) performing constant current density electrodeposition for a certain period of time; (4) After the electrodeposition is completed, the current collector is taken out and washed with water to obtain the Cl deposited on the current collector in situ. - Intercalated CoFe-LDH composite Ce(OH)3(CoFe-Cl - / Ce(OH)3) heterostructure catalytic electrode.

[0008] Preferably, the electrolyte solution in step (1) comprises: 0.02-0.1 M cobalt chloride hexahydrate, 0.01-0.05 M ferric nitrate nonahydrate, 0.01-0.05 M cerium nitrate hexahydrate, and 0.03-0.08 M ammonium chloride.

[0009] Preferably, the current collector in step (2) comprises an electrode material with excellent conductivity such as foamed nickel, foamed nickel-iron, foamed copper, stainless steel mesh, nickel foil, etc.

[0010] Preferably, the inert electrode plate in step (2) comprises an inert electrode material such as a graphite plate, a platinum plate, a silver plate, a gold plate, or a glassy carbon plate.

[0011] Preferably, in step (2), the distance between the current collector and the inert electrode plate is 7 to 20 mm.

[0012] Preferably, in step (2), the area of ​​the inert electrode plate is larger than the area of ​​the current collector.

[0013] Preferably, the certain time in step (3) is 1 to 60 minutes.

[0014] Preferably, the current density in step (3) is 1 to 300 mA cm -2 .

[0015] Compared with the existing preparation technology of anode catalyst for electrolysis of seawater, the synthesis method of the present invention has the following advantages: (1) mild synthesis conditions, short synthesis time, simple process flow, low cost, and large-scale production; (2) the CoFe-Cl synthesized by the method of the present invention is -The / Ce(OH)3 catalytic electrode is directly used as an anode catalytic electrode for electrolysis of seawater. On the one hand, no adhesive is needed during use, thereby effectively reducing the internal resistance of the electrode material; on the other hand, the catalytic electrode exhibits excellent OER catalytic activity and effectively resists Cl in seawater. - It can resist corrosion and has broad application prospects in the technology of hydrogen production by electrolysis of seawater. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The CoFe-Cl electrodeposited on nickel foam prepared in Example 1 - / XRD pattern of Ce(OH)3 catalytic electrode;

[0017] Figure 2 The CoFe-Cl electrodeposited on nickel foam prepared in Example 1 - / SEM image of Ce(OH)3 catalytic electrode;

[0018] Figure 3 The CoFe-Cl electrodeposited on nickel foam prepared in Example 1 - / Element distribution diagram of Ce(OH)3 catalytic electrode under TEM;

[0019] Figure 4 is the LSV performance diagram of the electrolysis of seawater anode OER of the catalytic electrodes prepared in Examples 1 to 3;

[0020] Figure 5 It is the LSV performance diagram of the electrolysis of seawater anode OER of the catalytic electrodes prepared in Example 1 and all comparative examples;

[0021] Figure 6 This is a stability performance diagram of the seawater electrolysis anode OER of the catalytic electrode prepared in Example 1. DETAILED DESCRIPTION

[0022] In order to illustrate the present invention in more detail, further description is given by specific implementation cases. The following examples do not limit the scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

[0023] Embodiment 1: (1) Accurately weigh 2.7 mmol of cobalt chloride hexahydrate, 1 mmol of ferric nitrate nonahydrate, 0.8 mmol of cerium nitrate hexahydrate, and 2.4 mmol of ammonium chloride, add them into 50 mL of deionized water, stir them thoroughly and dissolve them completely to obtain an electrolyte solution for electrodeposition; (2) using a dual counter electrode-single working electrode electrodeposition system, connecting a 1 cm×1 cm nickel foam and two 3 cm×3 cm graphite plates to the cathode and anode of a DC power supply, respectively, and immersing them in the electrolyte solution obtained in step (1); (3) At 120 mA cm -2 Electrodeposition at a constant current density of 4 min; (4) After the electrodeposition is completed, the nickel foam is taken out and washed with water to obtain Cl deposited on the nickel foam in situ. - Intercalated CoFe-LDH composite Ce(OH)3(CoFe-Cl - / Ce(OH)3) heterostructure catalytic electrode.

[0024] The prepared CoFe-Cl electrodeposited on nickel foam - / Ce(OH)3 as the working electrode, graphite rod as the counter electrode, and Hg / HgO electrode as the reference electrode to construct a three-electrode system to test the OER performance of the electrolytic seawater anode. The electrolyte is 1M KOH + seawater.

[0025] Embodiment 2: (1) Accurately weigh 2.7 mmol of cobalt chloride hexahydrate, 1 mmol of ferric nitrate nonahydrate, 0.6 mmol of cerium nitrate hexahydrate, and 2.4 mmol of ammonium chloride, add them into 50 mL of deionized water, stir them thoroughly and dissolve them completely to obtain an electrolyte solution for electrodeposition; (2) using a dual counter electrode-single working electrode electrodeposition system, connecting a 1 cm×1 cm nickel foam and two 3 cm×3 cm graphite plates to the cathode and anode of a DC power supply, respectively, and immersing them in the electrolyte solution obtained in step (1); (3) At 120 mA cm -2 Electrodeposition at a constant current density of 4 min; (4) After the electrodeposition is completed, the nickel foam is taken out and washed with water to obtain Cl deposited on the nickel foam in situ. - Intercalated CoFe-LDH composite Ce(OH)3(CoFe-Cl - / Ce(OH)3(0.6)) heterostructure catalytic electrode.

[0026] The method for testing the OER performance of the seawater electrolysis anode is the same as that in Example 1.

[0027] Embodiment 3: (1) Accurately weigh 2.7 mmol of cobalt chloride hexahydrate, 1 mmol of ferric nitrate nonahydrate, 1 mmol of cerium nitrate hexahydrate, and 2.4 mmol of ammonium chloride, add them into 50 mL of deionized water, stir them thoroughly and dissolve them completely to obtain an electrolyte solution for electrodeposition; (2) using a dual counter electrode-single working electrode electrodeposition system, connecting a 1 cm×1 cm nickel foam and two 3 cm×3 cm graphite plates to the cathode and anode of a DC power supply, respectively, and immersing them in the electrolyte solution obtained in step (1); (3) At 120 mA cm -2 Electrodeposition at a constant current density of 4 min; (4) After the electrodeposition is completed, the nickel foam is taken out and washed with water to obtain Cl deposited on the nickel foam in situ. - Intercalated CoFe-LDH composite Ce(OH)3(CoFe-Cl - / Ce(OH)3(1.0)) heterostructure catalytic electrode.

[0028] The method for testing the OER performance of the seawater electrolysis anode is the same as that in Example 1.

[0029] Comparative Example 1: (1) Accurately weigh 2.7 mmol of cobalt chloride hexahydrate, 1 mmol of ferric nitrate nonahydrate, and 2.4 mmol of ammonium chloride, add them into 50 mL of deionized water, stir them thoroughly and dissolve them completely to obtain an electrolyte solution for electrodeposition; (2) using a dual counter electrode-single working electrode electrodeposition system, connecting a 1 cm×1 cm nickel foam and two 3 cm×3 cm graphite plates to the cathode and anode of a DC power supply, respectively, and immersing them in the electrolyte solution obtained in step (1); (3) At 120 mA cm -2 Electrodeposition at a constant current density of 4 min; (4) After the electrodeposition is completed, the nickel foam is taken out and washed with water to obtain Cl deposited on the nickel foam in situ. - Intercalated CoFe-LDH (CoFe-Cl - ) catalytic electrode.

[0030] The method for testing the OER performance of the seawater electrolysis anode is the same as that in Example 1.

[0031] Comparative Example 2: (1) Accurately weigh 2.7 mmol of cobalt nitrate hexahydrate, 1 mmol of ferric nitrate nonahydrate, and 0.8 mmol of cerium nitrate hexahydrate, add them into 50 mL of deionized water, stir them thoroughly and dissolve them completely to obtain an electrolyte solution for electrodeposition; (2) using a dual counter electrode-single working electrode electrodeposition system, connecting a 1 cm×1 cm nickel foam and two 3 cm×3 cm graphite plates to the cathode and anode of a DC power supply, respectively, and immersing them in the electrolyte solution obtained in step (1); (3) At 120 mA cm -2 Electrodeposition at a constant current density of 4 min; (4) After the electrodeposition is completed, the nickel foam is taken out and washed with water to obtain NO3 in situ electrodeposited on the nickel foam. 2- Intercalated CoFe-LDH composite Ce(OH)3(CoFe-NO3 2- / Ce(OH)3) heterostructure catalytic electrode.

[0032] The method for testing the OER performance of the seawater electrolysis anode is the same as that in Example 1.

[0033] Comparative Example 3: (1) Accurately weigh 2.7 mmol of cobalt nitrate hexahydrate and 1 mmol of ferric nitrate nonahydrate, add them into 50 mL of deionized water, stir them thoroughly and dissolve them completely to obtain an electrolyte solution for electrodeposition; (2) using a dual counter electrode-single working electrode electrodeposition system, connecting a 1 cm×1 cm nickel foam and two 3 cm×3 cm graphite plates to the cathode and anode of a DC power supply, respectively, and immersing them in the electrolyte solution obtained in step (1); (3) At 120 mA cm -2 Electrodeposition at a constant current density of 4 min; (4) After the electrodeposition is completed, the nickel foam is taken out and washed with water to obtain NO3 in situ electrodeposited on the nickel foam. 2- Intercalated CoFe-LDH(CoFe-NO3 2 -) catalytic electrode.

[0034] The method for testing the OER performance of the seawater electrolysis anode is the same as that in Example 1.

[0035] Comparative Example 4: (1) Accurately weigh 0.8 mmol of cerium nitrate hexahydrate and add it to 50 mL of deionized water. Stir thoroughly and dissolve completely to obtain an electrolyte solution for electrodeposition; (2) using a dual counter electrode-single working electrode electrodeposition system, connecting a 1 cm×1 cm nickel foam and two 3 cm×3 cm graphite plates to the cathode and anode of a DC power supply, respectively, and immersing them in the electrolyte solution obtained in step (1); (3) At 120 mA cm -2 Electrodeposition at a constant current density of 4 min; (4) After the electrodeposition is completed, the nickel foam is taken out and washed with water to obtain a Ce(OH)3 catalytic electrode in situ electrodeposited on the nickel foam.

[0036] The method for testing the OER performance of the seawater electrolysis anode is the same as that in Example 1.

[0037] Figure 1: This is the XRD pattern of the material obtained in Example 1. The XRD pattern shows that the CoFe-LDH composite Ce(OH)3 heterostructure catalytic material is deposited on the nickel foam, and its diffraction angle is consistent with that of CoFe-LDH (PDF#50-0235) and Ce(OH)3 (PDF#19-0284).

[0038] Figure 2 This is a SEM image of the material obtained in Example 1. It can be seen that the catalytic material is deposited on the surface of the nickel foam in a textured manner.

[0039] Figure 3 The element distribution diagram of the material obtained in Example 1 under TEM shows that the Co, Fe, Ce, Cl, and O elements are evenly distributed, and there is no N element, indicating that CoFe-LDH has Cl - Intercalation.

[0040] Figure 4 The LSV diagrams of the OER of the catalytic materials prepared in Examples 1 to 3 are shown, wherein the material prepared in Example 1 exhibits the best anode OER performance for seawater electrolysis, achieving 1000 mA cm -2 At high current density, the overpotential is only 329mV.

[0041] Figure 5 The LSV diagrams of OER of the catalytic materials prepared in Example 1 and all comparative examples show that the catalytic material obtained in Example 1 exhibits the best catalytic activity.

[0042] Figure 6 The stability of the catalytic material prepared in Example 1 when applied to the anode for electrolysis of alkaline seawater is shown in Figure 1. -2 It has excellent stability and corrosion resistance for more than 200h at high current density.

Claims

1. A method for rapidly synthesizing a self-supporting corrosion-resistant anode catalyst for large current electrolysis of seawater at room temperature and pressure, characterized in that: The Cl-intercalated CoFe-LDH composite Ce(OH)3 heterostructure electrocatalytic material is in-situ electrodeposited on a current collector, and the synthesis method comprises the following steps: (1) Weighing cobalt chloride hexahydrate, ferric nitrate nonahydrate, cerium nitrate hexahydrate and ammonium chloride, adding them to deionized water, stirring them thoroughly to dissolve them completely to obtain an electrolyte solution for electrodeposition; (2) using a dual counter electrode-single working electrode electrodeposition system, connecting the current collector and the inert electrode plate to the cathode and anode of a DC power supply, respectively, and immersing them in the electrolyte solution obtained in step (1); (3) performing constant current density electrodeposition for a certain period of time; (4) After the electrodeposition is completed, the current collector is taken out and washed with water to obtain a Cl-intercalated CoFe-LDH composite Ce(OH)3 (CoFe-Cl- / Ce(OH)3) heterostructure catalytic electrode in situ electrodeposited on the current collector.

2. The method for rapidly synthesizing a self-supporting corrosion-resistant anode catalyst for large current electrolysis of seawater at room temperature and pressure as claimed in claim 1, characterized in that: The electrolyte solution in step (1) comprises: 0.02-0.1 M cobalt chloride hexahydrate, 0.01-0.05 M ferric nitrate nonahydrate, 0.01-0.05 M cerium nitrate hexahydrate, and 0.03-0.08 M ammonium chloride.

3. The method for rapidly synthesizing a self-supporting corrosion-resistant anode catalyst for large current electrolysis of seawater at room temperature and pressure as claimed in claim 1, characterized in that: The current collector in step (2) includes electrode materials with excellent conductivity such as foamed nickel, foamed nickel-iron, foamed copper, stainless steel mesh, and nickel foil.

4. The method for rapidly synthesizing a self-supporting corrosion-resistant anode catalyst for large current electrolysis of seawater at room temperature and pressure as claimed in claim 1, characterized in that: The inert electrode plate in step (2) includes inert electrode materials such as graphite plate, platinum plate, silver plate, gold plate, glassy carbon plate, etc.

5. The method for rapidly synthesizing a self-supporting corrosion-resistant anode catalyst for large current electrolysis of seawater at room temperature and pressure as claimed in claim 1, characterized in that: In step (2), the distance between the current collector and the inert electrode plate is 7 to 20 mm.

6. The method for rapidly synthesizing a self-supporting corrosion-resistant anode catalyst for large current electrolysis of seawater at room temperature and pressure as claimed in claim 1, characterized in that: In step (2), the area of ​​the inert electrode plate is larger than the area of ​​the current collector.

7. The method for rapidly synthesizing a self-supporting corrosion-resistant anode catalyst for large current electrolysis of seawater at room temperature and pressure as claimed in claim 1, characterized in that: The certain time in step (3) is 1 to 60 minutes.

8. The method for rapidly synthesizing a self-supporting corrosion-resistant anode catalyst for large current electrolysis of seawater at room temperature and pressure as claimed in claim 1, characterized in that: The current density in step (3) is 1 to 300 mA cm -2 .

Citation Information

Patent Citations

  • Preparation method of rare earth Ce doped NiCo-LDH electrocatalyst

    CN117568855A

Cited By

  • Rapid synthesis method of sulfate intercalation catalyst for seawater electrolysis hydrogen production

    CN119615258A

  • Preparation method of cerium hydroxide / nickel phosphide heterostructure catalyst for seawater electrolysis

    CN119843317A

  • Preparation method of cerium hydroxide / nickel phosphide heterostructure catalyst for seawater electrolysis

    CN119843317B