Carbon improver, phosphorus pig iron, graphite liquid and anode rod group
By using carbon improvers and phosphorus pig iron in the anode guide rod group, the conductivity of the anode is improved, the problem of insufficient conductivity of the anode is solved, the energy consumption of aluminum electrolytics is reduced, and an environmentally friendly production process is realized.
Patent Information
- Application Number
- CN202411541310.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-31
- Publication Date
- 2024-11-29
AI Technical Summary
In the prior art, the conductive performance between the anode steel claw and the anode carbon block is insufficiently improved, resulting in high energy consumption of electrolytic aluminum.
Carbon modified agent, phosphorus pig iron and graphite are used to improve the graphene surface through program heating and chemical vapor deposition technology, increase the number of carriers and conductivity, and add carbon modified agent to phosphorus pig iron to improve conductivity, forming Carbon-improved anode guide rod set.
It significantly improves the conductivity between the anode steel claw and the anode carbon block, reduces the energy consumption of aluminum electrolysis, and improves the smelting time and purity of phosphorus pig iron, and uses water to replace it. Kerosene improves environmental protection.
Smart Images

Figure CN119040966A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrolytic aluminum, and in particular to a carbon improver, phosphorus pig iron, graphite liquid and an anode guide rod assembly. Background Art
[0002] The anode of the aluminum electrolytic cell is one of the important raw materials for the production of electrolytic aluminum. It acts as a conductor to conduct direct current into the electrolyte layer, and at the same time, it participates in the anode reaction of electrolysis as a carbon material. At present, the production of one ton of electrolytic aluminum consumes about 13,000 to 14,000 kWh of electricity. Further reducing the energy consumption of electrolytic aluminum has always been an important research direction in the electrolytic aluminum industry. The energy consumption of electrolytic aluminum is mainly composed of the energy consumption of the anode part, the inter-electrode part, the cathode part and the busbar part. The prebaked anode is known as the "heart" of the electrolytic cell in the production of aluminum electrolysis. The entire anode voltage drop accounts for about 8% to 12% of the cell voltage. Therefore, improving the overall quality level of the anode, especially improving the conductivity of the anode, is the key to reducing the energy consumption per ton of aluminum. In the prior art, the anode part is mainly composed of three parts: the anode guide rod, the anode steel claw and the carbon block. The anode voltage drop energy consumption is very large. Further enhancing the conductivity of the anode carbon block is an effective way to reduce the energy consumption of aluminum electrolysis.
[0003] A Chinese invention patent application with publication number CN118621382A and publication date September 10, 2024 proposes an aluminum electrolysis anode and a method for preparing the same, wherein an aluminum electrolysis anode and a method for preparing the same are disclosed, wherein the material of the aluminum electrolysis anode includes carbon-based particles coated with a corrosion-resistant layer, the material of the carbon-based particles includes graphite, and the material of the corrosion-resistant layer includes graphene.
[0004] The principle is to set a corrosion-resistant layer on the surface of carbon-based particles. The corrosion-resistant layer protects the graphite surface in the carbon-based particles, which can significantly improve the corrosion resistance and oxidation resistance of the aluminum electrolysis anode. At the same time, since the material of the corrosion-resistant layer includes graphene, the corrosion-resistant layer also has good conductivity. Therefore, the present application achieves the balance of corrosion resistance, oxidation resistance and conductivity of the aluminum electrolysis anode.
[0005] With respect to the above technical solution, this type of material improves the anode carbon block, thereby enhancing the conductivity of the anode carbon block and reducing the energy consumption of electrolysis. However, the conductivity from the anode steel claw to the anode carbon block has not been improved, and the energy consumption of electrolysis is still very high. Summary of the invention
[0006] In order to improve the electrical conductivity between the anode steel claw and the anode carbon block, the present invention provides a carbon modifier, phosphorus pig iron, graphite liquid and an anode guide rod assembly.
[0007] In the first aspect, the present invention provides a carbon modifier and a preparation method thereof, which adopts the following technical scheme: A carbon modifier is prepared by the following steps: (1) Putting graphene into a porcelain boat and placing it in a tubular muffle furnace, heating the tube from room temperature to 500-800°C at a rate of 10-30°C / min by programmed temperature increase, pumping argon into the tube at a rate of 20 ml / min and oxygen at a rate of 30 ml / min, maintaining the pressure at 1 atmosphere, cooling to room temperature after reaching the temperature, turning off the oxygen during cooling, adjusting the argon to be pumped into the tube at a rate of 50 ml / min, maintaining the pressure at 1 atmosphere, and obtaining a precursor; (2) Using chemical vapor deposition, the precursor and titanium tetrachloride are mixed and placed in a vacuum tube furnace. The bottom of the tube furnace is evacuated to 5 Pa, and then hydrogen and argon are continuously introduced into the furnace chamber at 10 mL / min and 20 mL / min. At the same time, when the temperature rises to 450-650°C, it is kept warm for 10-45 minutes. After the reaction is completed, argon is kept introduced into the chamber, and the reaction is naturally cooled. The product is washed to obtain a carbon modifier.
[0008] By adopting the above technical solution, the graphene surface is first oxidized, and oxygen-containing functional groups are introduced on the graphene surface. These functional groups, as polar groups, can increase the polarity of the material surface, thereby increasing the number of carriers and improving the conductivity. Due to the oxygen-containing functional groups on the surface, it has good hydrophilicity and can form a stable dispersion in water; By means of programmed temperature increase, the reaction conditions can be precisely controlled to obtain the desired oxidation effect. By slowly increasing the temperature, the oxidation reaction can be made more uniform over the entire graphene surface.
[0009] Ti is loaded on the precursor by chemical vapor deposition to form Ti solid material on the surface of the precursor. The combination of the two changes the energy band structure of graphene. At the same time, the electron transmission property in the carbon modifier is excellent and the carrier mobility is very high, which enhances its conductive properties.
[0010] Optionally, the rate of programmed temperature increase in step (1) of the carbon modifier preparation method is 15-25°C / min.
[0011] Optionally, the heating temperature of the programmed temperature increase in step (1) of the carbon modifier preparation method is 600-750°C.
[0012] By adopting the above technical solution, the graphene can obtain a better oxidation effect by programmed heating at this rate and temperature, further improving its conductivity and hydrophilicity.
[0013] Optionally, the temperature of chemical vapor deposition in step (2) of the carbon modifier preparation method is 500-600°C.
[0014] Optionally, the time of chemical vapor deposition in step (2) of the carbon modifier preparation method is 20-35 minutes.
[0015] By adopting the above technical solution, TiCl4 can be decomposed more completely during chemical vapor deposition at this temperature and time, and graphene will not be damaged, resulting in a decrease in its conductive properties.
[0016] In a second aspect, the present invention provides a carbon-modified phosphorus pig iron, which comprises, by weight, 250-300 parts of phosphorus pig iron and 1-5 parts of a carbon modifier.
[0017] By adopting the above technical scheme, a carbon modifier is added to the phosphorus pig iron, and C and Ti in the carbon modifier are melted in the phosphorus pig iron, so that the melting time of the phosphorus pig iron is shortened and the plasticity is enhanced. During the casting process of the phosphorus pig iron, due to the addition of C and Ti, the ability of phosphorus to effectively absorb and remove impurities in the metal can be improved, which is helpful to improve the purity of aluminum. At the same time, it can play a role in refining the aluminum alloy grains, improving the fluidity of the aluminum liquid, reducing the resistance, and thus improving the electrolysis efficiency. The carbon modifier will not volatilize, and the phosphorus pig iron is a circulating material in the production system. The phosphorus iron ring can be enriched in the phosphorus pig iron system to achieve a better conductive effect.
[0018] In a third aspect, the present invention provides a carbon-modified graphite liquid, which comprises, by weight, 50-100 parts of graphite liquid and 1-5 parts of a carbon modifier, wherein the concentration of graphite in the graphite liquid is 10%, and the solvent is water.
[0019] By adopting the above technical scheme, the traditional method of dipping the anode steel claw in graphite is to mix graphite powder with kerosene, immerse the anode steel claw in the mixture of kerosene and graphite powder, and perform a graphite wet dipping operation. Since the dipping layer coated on the anode steel claw contains kerosene, when the anode is poured, the combustion of kerosene will produce flames and emit a large amount of black smoke, which will deteriorate the operating environment and cause environmental pollution. The addition of a carbon modifier and the introduction of oxygen-containing functional groups on the surface of the carbon modifier make the hydrophobic graphene itself have good hydrophilicity, and can form a stable dispersion in water. Water can be used instead of kerosene, which is more environmentally friendly.
[0020] In a fourth aspect, the present invention provides a carbon-modified anode guide rod assembly, which adopts the following technical solution: A carbon-modified anode guide rod assembly comprises a guide rod, a steel claw, a carbon-modified graphite liquid layer, a carbon-modified phosphorus pig iron layer and a carbon anode.
[0021] One end of the guide rod is connected to the steel claw, and the carbon-modified graphite liquid layer is wrapped outside the steel claw, and the carbon-modified graphite liquid layer is made of the carbon-modified graphite liquid described in the third aspect; the carbon-modified phosphorus pig iron layer is wrapped outside the carbon-modified graphite liquid layer, and the carbon-modified phosphorus pig iron layer is made of the carbon-modified phosphorus pig iron described in the second aspect; the carbon anode is connected to the carbon-modified phosphorus pig iron layer.
[0022] By adopting the above technical solution, the carbon-modified anode guide rod group can improve the conductivity between the anode steel claw and the anode carbon block, further enhance the conductivity of the anode carbon block, and reduce the energy consumption of aluminum electrolysis.
[0023] In summary, the present invention includes at least one of the following beneficial technical effects: The carbon-modified anode guide rod assembly can improve the electrical conductivity between the anode steel claw and the anode carbon block, further enhance the electrical conductivity of the anode carbon block, and reduce the energy consumption of aluminum electrolysis.
[0024] A carbon modifier is added to phosphorus pig iron, and C and Ti in the carbon modifier are melted in the phosphorus pig iron, which shortens the melting time of the phosphorus pig iron and enhances its plasticity. During the casting process of the phosphorus pig iron, the addition of C and Ti can enhance the ability of phosphorus to effectively absorb and remove impurities in the metal, which helps to improve the purity of aluminum. At the same time, it can refine the aluminum alloy grains, improve the fluidity of the aluminum liquid, reduce resistance, and thus improve the electrolysis efficiency. The carbon modifier will not volatilize, and the phosphorus pig iron is a circulating material in the production system. The phosphorus-iron ring can be enriched in the phosphorus pig iron system to achieve a better conductive effect.
[0025] A carbon modifier is added to the graphite liquid. Oxygen-containing functional groups are introduced on the surface of the carbon modifier, which makes the hydrophobic graphene itself have good hydrophilicity and can form a stable dispersion in water. Water can be used instead of kerosene, which is more environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic diagram of the overall structure of the present invention; Explanation of the reference numerals: 1. guide rod; 2. steel claw; 3. carbon-modified graphite liquid layer; 4. carbon-modified phosphorus pig iron layer; 5. carbon anode. DETAILED DESCRIPTION
[0027] The present invention is further described in detail below with reference to the embodiments.
[0028] The phosphorus pig iron is ordinary ferrophosphorus FeP24 produced by Henan Huijin Metallurgical Technology Co., Ltd.
[0029] Example 1: This example discloses a carbon-modified anode guide rod assembly, which includes a guide rod 1, a steel claw 2, a carbon-modified graphite liquid layer 3, a carbon-modified phosphorus pig iron layer 4, and a carbon anode 5.
[0030] One end of the guide rod 1 is connected to the steel claw 2 , and the carbon-modified graphite liquid layer 3 is wrapped outside the steel claw 2 ; the carbon-modified phosphorus pig iron layer 4 is wrapped outside the carbon-modified graphite liquid layer 3 ; and the carbon anode 5 is connected to the carbon-modified phosphorus pig iron layer 4 .
[0031] The carbon modified graphite liquid comprises, by weight, 50-100 parts of graphite liquid and 1-5 parts of carbon modifier, wherein the concentration of graphite in the graphite liquid is 10%, and the solvent is water.
[0032] The carbon-modified phosphorus pig iron comprises, by weight, 250-300 parts of phosphorus pig iron and 1-5 parts of a carbon modifier.
[0033] A carbon modifier is prepared by the following steps: (1) Putting graphene into a porcelain boat and placing it in a tubular muffle furnace, heating the tube from room temperature to 500-800°C at a rate of 10-30°C / min by programmed temperature increase, pumping argon into the tube at a rate of 20 ml / min and oxygen at a rate of 30 ml / min, maintaining the pressure at 1 atmosphere, cooling to room temperature after reaching the temperature, turning off the oxygen during cooling, adjusting the argon to be pumped into the tube at a rate of 50 ml / min, maintaining the pressure at 1 atmosphere, and obtaining a precursor; (2) Using chemical vapor deposition, the precursor and titanium tetrachloride are mixed and placed in a vacuum tube furnace. The bottom of the tube furnace is evacuated to 5 Pa, and then hydrogen and argon are continuously introduced into the furnace chamber at 10 mL / min and 20 mL / min. At the same time, when the temperature rises to 450-650°C, it is kept warm for 10-45 minutes. After the reaction is completed, argon is kept introduced into the chamber, and the reaction is naturally cooled. The product is washed to obtain a carbon modifier.
[0034] After the carbon modifier is added into the graphite liquid and fully dissolved, the carbon-modified graphite liquid is dipped with a steel claw 2 to obtain a carbon-modified graphite liquid layer 3; the carbon modifier is then added into the molten phosphorus pig iron to obtain the carbon-modified phosphorus pig iron for casting the carbon anode 5 to obtain a carbon-modified phosphorus pig iron layer 4, and after cooling, a carbon-modified anode guide rod group is obtained.
[0035] Example 2: This example discloses a carbon-modified anode guide rod assembly. Step (1) in the method for preparing the carbon-modifying agent is different from that in Example 1, and the rest is the same as that in Example 1.
[0036] The preparation method of the carbon improver is as follows: (1) Graphene was placed in a porcelain boat in a tubular muffle furnace, and the tube was heated from room temperature to 750°C at a rate of 25°C / min by programmed temperature increase.
[0037] Example 3: This example discloses a carbon-modified anode guide rod assembly. Step (1) in the method for preparing the carbon-modifying agent is different from that in Example 1, and the rest is the same as that in Example 1.
[0038] The preparation method of the carbon modifier is as follows: (2) Using chemical vapor deposition, when the temperature rises to 450°C, keep it warm for 10 minutes.
[0039] Comparative Example 1: This comparative example discloses a carbon-modified anode guide rod assembly, which includes a guide rod 1, a steel claw 2, a carbon-modified graphite liquid layer 3, a carbon-modified phosphorus pig iron layer 4, and a carbon anode 5.
[0040] One end of the guide rod 1 is connected to the steel claw 2 , and the carbon-modified graphite liquid layer 3 is wrapped outside the steel claw 2 ; the carbon-modified phosphorus pig iron layer 4 is wrapped outside the carbon-modified graphite liquid layer 3 ; and the carbon anode 5 is connected to the carbon-modified phosphorus pig iron layer 4 .
[0041] The carbon modified graphite liquid comprises, by weight, 50-100 parts of graphite liquid and 1-5 parts of carbon modifier, wherein the concentration of graphite in the graphite liquid is 10%, and the solvent is water.
[0042] The carbon-modified phosphorus pig iron comprises, by weight, 250-300 parts of phosphorus pig iron and 1-5 parts of a carbon modifier.
[0043] A carbon modifier is prepared by the following steps: Put graphene into a porcelain boat and place it in a tubular muffle furnace. Heat the tube from room temperature to 650°C at a rate of 20°C / min by programmed temperature increase. Pump argon into the tube at a rate of 20 ml / min and oxygen at a rate of 30 ml / min. Maintain the pressure at 1 atmosphere. After reaching the temperature, cool to room temperature. During cooling, turn off the oxygen. Adjust argon to be pumped into the tube at a rate of 50 ml / min. Maintain the pressure at 1 atmosphere to obtain a precursor. After the carbon modifier is added into the graphite liquid and fully dissolved, the carbon-modified graphite liquid is dipped with a steel claw 2 to obtain a carbon-modified graphite liquid layer 3; the carbon modifier is then added into the molten phosphorus pig iron to obtain the carbon-modified phosphorus pig iron for casting the carbon anode 5 to obtain a carbon-modified phosphorus pig iron layer 4, and after cooling, a carbon-modified anode guide rod group is obtained.
[0044] Comparative Example 2: This comparative example discloses a carbon-modified anode guide rod assembly, which includes a guide rod 1, a steel claw 2, a carbon-modified graphite liquid layer, a carbon-modified phosphorus pig iron layer, and a carbon anode 5.
[0045] One end of the guide rod 1 is connected to the steel claw 2 , and the carbon-modified graphite liquid layer 3 is wrapped outside the steel claw 2 ; the carbon-modified phosphorus pig iron layer 4 is wrapped outside the carbon-modified graphite liquid layer 3 ; and the carbon anode 5 is connected to the carbon-modified phosphorus pig iron layer 4 .
[0046] The carbon modified graphite liquid comprises, by weight, 50-100 parts of graphite liquid and 1-5 parts of carbon modifier, wherein the concentration of graphite in the graphite liquid is 10%, and the solvent is water.
[0047] The carbon-modified phosphorus pig iron comprises, by weight, 250-300 parts of phosphorus pig iron and 1-5 parts of a carbon modifier.
[0048] A carbon modifier is prepared by the following steps: The precursor and titanium tetrachloride were mixed by chemical vapor deposition and placed in a vacuum tube furnace. The bottom vacuum of the tube furnace was evacuated to 5 Pa, and then hydrogen and argon were continuously introduced into the furnace chamber at 10 mL / min and 20 mL / min. At the same time, when the temperature was raised to 550°C, it was kept warm for 15 minutes. After the reaction was completed, argon was kept introduced into the chamber, and the mixture was naturally cooled and the product was washed to obtain a carbon modifier.
[0049] After the carbon modifier is added into the graphite liquid and fully dissolved, the carbon-modified graphite liquid is dipped with a steel claw 2 to obtain a carbon-modified graphite liquid layer 3; the carbon modifier is then added into the molten phosphorus pig iron to obtain the carbon-modified phosphorus pig iron for casting the carbon anode 5 to obtain a carbon-modified phosphorus pig iron layer 4, and after cooling, a carbon-modified anode guide rod group is obtained.
[0050] Comparative Example 3: This comparative example discloses an anode guide rod assembly, which includes a guide rod, a steel claw, a graphite solution, phosphorus pig iron, and a carbon anode, wherein the concentration of graphite in the graphite solution is 10%, and the solvent is water.
[0051] One end of the guide rod is connected to a steel claw, and a graphite liquid layer is wrapped outside the steel claw; the phosphorus pig iron layer is wrapped outside the graphite liquid layer; and the carbon anode is connected to the phosphorus pig iron layer.
[0052] The graphite liquid is dipped with a steel claw; then the molten phosphorus pig iron is used to cast the carbon anode to obtain the anode guide rod assembly.
[0053] The anode guide rod groups prepared in Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, and Comparative Example 3 were tested and experimented.
[0054]
[0055] By comparing Example 1 with Comparative Example 3, it can be seen that the carbon-modified anode guide rod assembly can effectively reduce the energy consumption of aluminum electrolysis.
[0056] By comparing Example 1 with Example 2, it can be seen that by increasing the temperature and heating time of the programmed heating, the increased temperature and time will cause defects in the structure of the graphene, and the energy consumption is reduced, but it is within an acceptable range.
[0057] By comparing Example 1 with Example 3, it can be seen that by reducing the temperature and holding time of chemical vapor deposition, the decomposition of TiCl4 is not complete, the Ti loading is too low, the conductivity is reduced, and the energy consumption is reduced, but it is within an acceptable range.
[0058] By comparing Example 1 with Comparative Example 1, it can be seen that by reducing the step of programmed temperature rise, the surface of the carbon modifier lacks oxygen-containing functional groups and cannot form a stable dispersion in water. When dipping graphite, it cannot be evenly dispersed on the anode steel claw, the amount of dipping is small, the conductivity is reduced, and the energy consumption is reduced.
[0059] By comparing Example 1 with Comparative Example 2, it can be seen that by reducing the chemical vapor deposition step, there is no Ti load, the conductivity is reduced, and the energy consumption is reduced.
[0060] The above are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A carbon modifier, characterized in that: The method comprises the following steps: (1) Putting graphene into a porcelain boat and placing it in a tubular muffle furnace, heating the tube from room temperature to 500-800°C at a rate of 10-30°C / min by programmed temperature increase, pumping argon into the tube at a rate of 20 ml / min and oxygen at a rate of 30 ml / min, maintaining the pressure at 1 atmosphere, cooling to room temperature after reaching the temperature, turning off the oxygen during cooling, adjusting the argon to be pumped into the tube at a rate of 50 ml / min, maintaining the pressure at 1 atmosphere, and obtaining a precursor; (2) Using chemical vapor deposition, the precursor and titanium tetrachloride are mixed and placed in a vacuum tube furnace. The bottom of the tube furnace is evacuated to 5 Pa, and then hydrogen and argon are continuously introduced into the furnace chamber at 10 ml / min and 20 ml / min. At the same time, when the temperature rises to 450-650°C, it is kept warm for 10-45 minutes. After the reaction is completed, argon is kept introduced into the chamber, and the chamber is naturally cooled and the product is washed to obtain a carbon modifier.
2. The method of preparing a carbon modifier according to claim 1, characterized in that: The rate of programmed temperature increase in step (1) of the carbon modifier preparation method is 15-25°C / min.
3. The method of preparing a carbon modifier according to claim 1, characterized in that: The heating temperature of the programmed temperature rise in step (1) of the carbon modifier preparation method is 600-750°C.
4. The method of preparing a carbon modifier according to claim 1, characterized in that: The temperature of chemical vapor deposition in step (2) of the carbon modifier preparation method is 500-600°C.
5. The method of preparing a carbon modifier according to claim 1, characterized in that: The time of chemical vapor deposition in step (2) of the carbon modifier preparation method is 20-35 minutes.
6. A carbon-modified phosphorus pig iron, characterized in that: The composition comprises, by weight, 250-300 parts of phosphorus pig iron and 1-5 parts of the carbon improver described in any one of claims 1-5.
7. A carbon-modified graphite liquid, characterized in that: The composition comprises, by weight: 50-100 parts of graphite liquid and 1-5 parts of any one of claims 1-5 carbon improvers, wherein the concentration of graphite in the graphite liquid is 10%, and the solvent is water.
8. A carbon-modified anode guide rod assembly, comprising a guide rod (1), a steel claw (2), a carbon-modified graphite liquid layer (3), a carbon-modified phosphorus pig iron layer (4), and a carbon anode (5); One end of the guide rod (1) is connected to the steel claw (2), the carbon-modified graphite liquid layer (3) is wrapped around the outside of the steel claw (2), and the carbon-modified graphite liquid layer (3) is made of the carbon-modified graphite liquid described in claim 7; the carbon-modified phosphorus pig iron layer (4) is wrapped around the outside of the carbon-modified graphite liquid layer (3), and the carbon-modified phosphorus pig iron layer (4) is made of the carbon-modified phosphorus pig iron described in claim 6; the carbon anode (5) is connected to the carbon-modified phosphorus pig iron layer (4).
Citation Information
Patent Citations
Aluminum electrolysis anode and preparation method thereof
CN118621382A