Preparation method of photo-thermal conversion yarn

By forming composite structures such as tungsten trioxide, zirconium carbide, carbon nanotubes, etc. and combining them with polyvinyl alcohol, the photothermal conversion yarn is prepared by laser drying, which solves the problem of low efficiency of existing photothermal conversion yarns. It achieves efficient photothermal conversion and temperature regulation effects.

CN119041205APending Publication Date: 2024-11-29沪本新材料科技(上海)有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411288438.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing photothermal conversion yarns have low photothermal conversion efficiency, making it difficult to meet the demand for efficient temperature regulation in many fields.

Method used

By ball milling, grinding, ultrasonic, lyophilizing and chemical reactions of materials such as tungsten trioxide, zirconium carbide, carbon nanotubes, graphene oxide, silicon carbide and rare earth oxides, forming a composite structure and combining it with polyvinyl alcohol. The laser drying method prepares photothermal conversion yarns to improve the uniform distribution and heat conduction properties of the material.

Benefits of technology

The photothermal conversion efficiency of the photothermal conversion yarn is significantly improved, its mechanical strength and toughness are enhanced, and its performance can be maintained in harsh environments and efficient temperature regulation is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a preparation method of photo-thermal conversion yarn, and belongs to the technical field of photo-thermal conversion material preparation. Tungsten trioxide, zirconium carbide and carbon nanotubes are combined with graphene oxide through a freeze-drying method to prepare a composite structure, and then the composite structure, silicon carbide subjected to surface pretreatment and rare earth oxide are further ground and mixed to prepare the photothermal conversion composite material. Multiple components in the composite material can absorb ultraviolet rays, near-infrared rays and far-infrared rays through a synergistic effect and effectively convert the ultraviolet rays, the near-infrared rays and the far-infrared rays into heat energy; according to the invention, polyvinyl alcohol is used as an adhesive and a base material, and the photothermal conversion composite material is uniformly dispersed in the polyvinyl alcohol by stirring to form a stable compound. Firstly, yarn is soaked and heated, so that the surface of the yarn is cleaner and more activated, attachment of a subsequent coating is facilitated, then the pretreated yarn is coated with the compound, rapid drying is conducted through a laser drying method, and the photo-thermal conversion yarn is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photothermal conversion material preparation, and relates to a method for preparing photothermal conversion yarn. Background Art

[0002] Photothermal conversion refers to the process of converting light energy into heat energy. In photothermal conversion yarn, this principle is cleverly applied to the yarn material. By coating or embedding special photothermal conversion materials on the surface of the yarn, when light shines on the yarn, these materials can absorb light energy and convert it into heat energy, thereby increasing the temperature of the yarn. This conversion process makes it possible for yarn to be used in many fields.

[0003] Photothermal-electric conversion smart textiles can give textiles more functions by converting light energy into heat energy. They can adjust the temperature of textiles in real time according to the ambient temperature to achieve intelligent warmth or cooling. As a new type of material, photothermal conversion yarn has made significant progress in the principle of photothermal conversion, yarn material innovation, and application fields. With the continuous development and improvement of technology, photothermal conversion yarn is expected to play an important role in more fields and bring more convenience and comfort to human life. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing a photothermal conversion yarn, which has the characteristics of high photothermal conversion efficiency.

[0005] The purpose of the present invention can be achieved through the following technical solutions: A method for preparing a photothermal conversion yarn, the process of preparing the photothermal conversion yarn is as follows: S1: tungsten trioxide, zirconium carbide and carbon nanotubes are mixed in a mass ratio of (3-5):1:2, and ground in a ball mill at a speed of 500 r / min for 1-2 h to obtain a mixture A; S2: dissolving graphene oxide in deionized water to obtain a graphene oxide solution with a mass fraction of 30-50%, dispersing mixture A in the graphene oxide solution, wherein the mass ratio of mixture A to graphene oxide is 1:(1-3), and ultrasonicating for 0.5-2h to obtain a solid-liquid mixture B; S3: freeze-dry the solid-liquid mixture after ultrasound in liquid nitrogen for 10-15 min, and then dry it at -50--30°C for 4-6 h, and grind the solid obtained after freeze-drying to obtain a mixture C; S4: A 20% by mass hydrogen peroxide solution and a 20% by mass sulfuric acid solution are mixed in a volume ratio of 1:1 to obtain a mixed solution, silicon carbide is dispersed in the mixed solution, heated to 50°C, stirred at a speed of 150 r / min for 2-3 hours to obtain a solid-liquid mixture with a mass fraction of 20-30%, and after the reaction is completed, slowly cooled to room temperature, filtered and washed to obtain a mixture D; S5: Mix the mixture C and the mixture D in a mass ratio of (1-3):1, add 2-3 wt% of rare earth oxide, and grind in a ball mill at a speed of 500-600 r / min for 1-2 h to obtain a mixture E; S6: heating the polyvinyl alcohol to 75-85° C., stirring at a speed of 200 r / min, adding mixture E while stirring, wherein the mass ratio of mixture E to polyvinyl alcohol is 1:1, and then adding 0.5-1wt% of a dispersant, stirring for 2-3 h, to obtain mixture F; S7: soaking the yarn in deionized water, heating to 100°C, reacting for 2-3 hours, taking out the yarn, and drying it at 110°C for 24 hours; S8: Use nitrogen to purge the dried yarn, and immerse the purged yarn in the mixture F for 6 to 8 hours at a temperature of 80°C. After the immersion is completed, use a laser drying method to dry the yarn to obtain the photothermal conversion yarn.

[0006] Furthermore, the particle size of the mixture A in S1 is 200 mesh.

[0007] Furthermore, the particle size of the mixture C in S3 is 200 mesh.

[0008] Furthermore, the cooling rate in S4 is 2°C / min.

[0009] Furthermore, the rare earth oxide in S5 is one or more of cerium oxide, lanthanum oxide, praseodymium oxide, and rubidium oxide.

[0010] Furthermore, the dispersant in S6 is polyethylene glycol, and its number average molecular weight is 2000-10000.

[0011] Furthermore, the purge flow rate of nitrogen in S8 is 8-10 m / s.

[0012] Furthermore, the parameters of the laser drying method in S8 are: laser power 300W, temperature 60°C, and irradiation time 30min.

[0013] The photothermal conversion yarn prepared by the present invention, when light irradiates the yarn surface, the photothermal conversion material in the yarn absorbs light energy and converts it into heat energy, thereby increasing the temperature of the yarn. In the preparation process of the present invention, various functional materials are uniformly coated or embedded on the yarn surface through physical means such as ball milling, grinding and ultrasound, as well as chemical reactions, to form a stable physical and chemical combination.

[0014] Tungsten trioxide is an important semiconductor material with excellent photoelectric properties and thermal stability. In the process of light-to-heat conversion, it can effectively absorb ultraviolet rays and part of visible light in sunlight and convert them into thermal energy. In addition, the band gap width of tungsten trioxide is moderate, which makes it have a high light absorption efficiency within a certain wavelength range. In the preparation process of the present invention, tungsten trioxide is used as the main light-absorbing material to provide the yarn with efficient light-to-heat conversion ability.

[0015] Zirconium carbide is a ceramic material with a high melting point and high hardness, and has good thermal conductivity and mechanical properties. In the preparation of photothermal conversion yarn, the addition of zirconium carbide can further enhance the thermal conductivity of the yarn, so that the absorbed light energy can be transferred to various parts of the yarn more quickly, thereby improving the overall photothermal conversion efficiency.

[0016] Carbon nanotubes have an extremely high aspect ratio, excellent electrical conductivity and thermal conductivity, and good mechanical properties. In the preparation of photothermal conversion yarns, carbon nanotubes can be used as heat conduction channels to enhance the thermal conductivity of the yarns, allowing heat energy to be transferred and diffused faster, improving the mechanical strength and toughness of the yarns, and enabling the yarns to withstand greater external forces and wear in practical applications. Carbon nanotubes also have a nano effect, through which they form a close bond with other photothermal conversion materials in the yarns, thereby improving the overall performance of the yarns.

[0017] Tungsten trioxide absorbs light energy and converts it into heat energy, while zirconium carbide and carbon nanotubes act as heat conduction channels to quickly transfer heat energy to various parts of the yarn, thereby improving the light-to-heat conversion efficiency; the high hardness and high strength of zirconium carbide and carbon nanotubes provide additional mechanical support for the yarn, making it less likely to break or deform when subjected to external forces; the combination of the three improves the thermal and chemical stability of the yarn, allowing the yarn to maintain its performance in various harsh environments.

[0018] As a two-dimensional nanomaterial, graphene oxide has excellent thermal conductivity and light absorption capacity. In the process of photothermal conversion, it can effectively absorb light energy and convert it into heat energy, thereby improving the photothermal conversion efficiency of the yarn. Graphene oxide also has good dispersibility and stability, which can help nanomaterials such as tungsten trioxide, zirconium carbide and carbon nanotubes to be evenly dispersed in the solution and prevent them from agglomerating. This uniform dispersion state is conducive to the uniform distribution of nanomaterials in the yarn, thereby further improving the photothermal conversion performance of the yarn.

[0019] By dispersing tungsten trioxide, zirconium carbide and carbon nanotubes in a graphene oxide solution and freeze-drying them, several photothermal conversion materials can form a more compact composite structure. This composite structure helps the synergistic effect between the nanomaterials, thereby improving the photothermal conversion performance of the yarn.

[0020] Silicon carbide is a highly thermally conductive material with good thermal conductivity. In photothermal conversion yarns, the addition of silicon carbide can improve the overall thermal conductivity of the yarn, so that the yarn can transfer heat energy to other parts of the yarn more quickly after absorbing light energy, thereby improving the photothermal conversion efficiency. It can form a composite structure with photothermal conversion materials such as tungsten trioxide, zirconium carbide, and carbon nanotubes in the yarn. This composite structure helps to absorb, transfer and convert light energy, thereby improving the photothermal conversion efficiency of the yarn. Silicon carbide has excellent chemical stability and thermal stability, and can maintain its performance unchanged under high temperature and harsh environments. The present invention first pre-treats silicon carbide with a mixed solution of hydrogen peroxide and sulfuric acid, and the mixed solution has strong oxidizing properties and can oxidize the surface of silicon carbide. This oxidation will change the surface chemical properties of silicon carbide and increase the hydroxyl or other oxygen-containing functional groups on the surface. The presence of these functional groups helps to enhance the interaction between silicon carbide and other materials and improve the overall performance of the composite material. During the preparation and use of the photothermal conversion yarn of the present invention, the addition of pretreated silicon carbide can improve the overall stability of the yarn and prevent the yarn from thermal decomposition or performance degradation at high temperatures.

[0021] In addition, the surface of the oxidized silicon carbide becomes more hydrophilic, which helps it to be better dispersed in polyvinyl alcohol in the subsequent steps, ensuring that the silicon carbide particles can be evenly distributed in the yarn matrix.

[0022] Rare earth elements have special optical properties. Their electronic structure and energy level distribution enable rare earth oxides to absorb light of specific wavelengths. In photothermal conversion yarns, the addition of rare earth oxides can significantly enhance the yarn's ability to absorb light energy, allowing more light energy to be captured by the yarn and converted into heat energy. Rare earth oxides can not only absorb light energy, but also undergo processes such as photoluminescence and photoheating inside them, efficiently converting the absorbed light energy into heat energy. Rare earth oxides can work in synergy with other components to improve the yarn's light absorption, photothermal conversion, and heat energy transfer capabilities by changing the surface properties of other components, optimizing their band structures, or promoting the separation and transmission of photogenerated carriers.

[0023] In addition, when rare earth oxides are mixed and ground with tungsten trioxide, zirconium carbide and carbon nanotubes, a large number of interfaces are formed between them. These interfaces are areas where physical and chemical properties suddenly change, and are also important places for energy conversion and transfer. Rare earth oxides are first adsorbed on the surface of other materials and gradually penetrate into the interior of the materials through diffusion. During the adsorption and diffusion process, rare earth oxides interact with electrons in other materials, resulting in changes in electronic structure and redistribution of charge. At the interface, rare earth oxides will react chemically with other materials to form new chemical bonds. These interfacial reactions will change the physical and chemical properties of the materials.

[0024] Therefore, the present invention first combines tungsten trioxide, zirconium carbide and carbon nanotubes with graphene oxide through a freeze-drying method to obtain a composite structure, and then further grinds and mixes them with silicon carbide and rare earth oxides after surface pretreatment to obtain a photothermal conversion composite material. The multiple components in the composite material can absorb ultraviolet, near-infrared and far-infrared through a synergistic effect and effectively convert them into thermal energy.

[0025] The present invention uses polyvinyl alcohol as an adhesive and a matrix material, and disperses the photothermal conversion composite material uniformly therein by stirring to form a stable composite material. The yarn is first treated by soaking and heating to make its surface cleaner and activated, which is conducive to the attachment of subsequent coatings. The composite material is then coated on the pretreated yarn and quickly dried by laser drying to obtain a photothermal conversion yarn. Laser drying uses the high energy density of the laser beam to quickly heat the coating surface, causing the water to evaporate rapidly, thereby achieving rapid drying.

[0026] Beneficial effects of the present invention: (1) In the present invention, tungsten trioxide, zirconium carbide and carbon nanotubes are first combined with graphene oxide by freeze-drying to obtain a composite structure, and then further ground and mixed with silicon carbide and rare earth oxide after surface pretreatment to obtain a light-to-heat conversion composite material. The multiple components in the composite material can absorb ultraviolet, near-infrared and far-infrared through synergistic effects and effectively convert them into heat energy; (2) The present invention uses polyvinyl alcohol as an adhesive and a matrix material, and disperses the photothermal conversion composite material uniformly therein by stirring to form a stable composite material. The yarn is first treated by soaking and heating to make its surface cleaner and more activated, which is conducive to the attachment of the subsequent coating. The composite material is then coated on the pretreated yarn and quickly dried by laser drying to obtain the photothermal conversion yarn. DETAILED DESCRIPTION

[0027] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0028] Example 1 S1: tungsten trioxide, zirconium carbide and carbon nanotubes were mixed in a mass ratio of 4:1:2, and ground in a ball mill at a speed of 500 r / min for 1.5 h to obtain a mixture A, wherein the particle size of the mixture A was 200 meshes; S2: dissolving graphene oxide in deionized water to obtain a graphene oxide solution with a mass fraction of 40%, dispersing mixture A in the graphene oxide solution, wherein the mass ratio of mixture A to graphene oxide is 1:2, and ultrasonicating for 1 h to obtain a solid-liquid mixture B; S3: The solid-liquid mixture after ultrasonication is placed in liquid nitrogen for freeze-drying for 15 minutes, and then dried at -50°C for 4 hours, and the solid obtained after freeze-drying is crushed and ground to obtain a mixture C, wherein the particle size of the mixture C is 200 mesh; S4: A 20% by mass hydrogen peroxide solution and a 20% by mass sulfuric acid solution were mixed in a volume ratio of 1:1 to obtain a mixed solution, silicon carbide was dispersed in the mixed solution, heated to 50°C, stirred at a speed of 150 r / min for 2 hours to obtain a solid-liquid mixture with a mass fraction of 30%, and after the reaction was completed, the mixture was slowly cooled to room temperature at a cooling rate of 2°C / min, filtered and washed to obtain a mixture D; S5: Mixture C and mixture D in a mass ratio of 2:1, add 3 wt % cerium oxide, and grind in a ball mill at a speed of 600 r / min for 1 h to obtain mixture E; S6: heating the polyvinyl alcohol to 80° C., stirring at a speed of 200 r / min, adding mixture E while stirring, wherein the mass ratio of mixture E to polyvinyl alcohol is 1:1, and then adding 1 wt % of polyethylene glycol 5000, stirring for 3 h, to obtain mixture F; S7: soaking the yarn in deionized water, heating to 100°C, reacting for 3 hours, taking out the yarn, and drying it at 110°C for 24 hours; S8: Use nitrogen to purge the dried yarn, the nitrogen purge flow rate is 9m / s, and the purged yarn is immersed in the mixture F for 7h at a temperature of 80°C. After the immersion is completed, the yarn is dried by a laser drying method. The parameters of the laser drying method are laser power 300W, temperature 60°C, and irradiation time 30min to obtain the photothermal conversion yarn.

[0029] Example 2 S1: Tungsten trioxide, zirconium carbide and carbon nanotubes were mixed in a mass ratio of 3:1:2, and ground in a ball mill at a speed of 500 r / min for 1 h to obtain a mixture A, wherein the particle size of the mixture A was 200 meshes; S2: dissolving graphene oxide in deionized water to obtain a graphene oxide solution with a mass fraction of 30%, dispersing mixture A in the graphene oxide solution, wherein the mass ratio of mixture A to graphene oxide is 1:1, and ultrasonicating for 0.5 h to obtain a solid-liquid mixture B; S3: The solid-liquid mixture after ultrasonication is placed in liquid nitrogen for freeze-drying for 10 minutes, and then dried at -50°C for 4 hours, and the solid obtained after freeze-drying is crushed and ground to obtain a mixture C, wherein the particle size of the mixture C is 200 mesh; S4: A 20% by mass hydrogen peroxide solution and a 20% by mass sulfuric acid solution were mixed in a volume ratio of 1:1 to obtain a mixed solution, silicon carbide was dispersed in the mixed solution, heated to 50°C, stirred at a speed of 150 r / min for 2 hours to obtain a solid-liquid mixture with a mass fraction of 20%, and after the reaction was completed, the mixture was slowly cooled to room temperature at a cooling rate of 2°C / min, filtered and washed to obtain a mixture D; S5: Mixture C and mixture D in a mass ratio of 1:1, add 2 wt % lanthanum oxide, and grind in a ball mill at a speed of 500 r / min for 1 h to obtain mixture E; S6: heating the polyvinyl alcohol to 75° C., stirring at a speed of 200 r / min, adding mixture E while stirring, wherein the mass ratio of mixture E to polyvinyl alcohol is 1:1, and then adding 0.5 wt % of polyethylene glycol 2000, stirring for 2 h, to obtain mixture F; S7: soaking the yarn in deionized water, heating to 100°C, reacting for 2 hours, taking out the yarn, and drying it at 110°C for 24 hours; S8: Use nitrogen to purge the dried yarn, the purge flow rate of nitrogen is 8m / s, and the purged yarn is immersed in mixture F for 6h at a temperature of 80°C. After the immersion is completed, the yarn is dried by a laser drying method. The parameters of the laser drying method are laser power 300W, temperature 60°C, and irradiation time 30min to obtain the photothermal conversion yarn.

[0030] Example 3 S1: Tungsten trioxide, zirconium carbide and carbon nanotubes were mixed in a mass ratio of 5:1:2, and ground in a ball mill at a speed of 500 r / min for 2 h to obtain a mixture A, wherein the particle size of the mixture A was 200 meshes; S2: dissolving graphene oxide in deionized water to obtain a graphene oxide solution with a mass fraction of 30-50%, dispersing mixture A in the graphene oxide solution, wherein the mass ratio of mixture A to graphene oxide is 1:3, and ultrasonicating for 2 h to obtain a solid-liquid mixture B; S3: The solid-liquid mixture after ultrasonication is placed in liquid nitrogen for freeze-drying for 15 minutes, and then dried at -30°C for 6 hours, and the solid obtained after freeze-drying is crushed and ground to obtain a mixture C, wherein the particle size of the mixture C is 200 mesh; S4: A 20% by mass hydrogen peroxide solution and a 20% by mass sulfuric acid solution were mixed in a volume ratio of 1:1 to obtain a mixed solution, silicon carbide was dispersed in the mixed solution, heated to 50°C, stirred at a speed of 150 r / min for 2-3 hours to obtain a solid-liquid mixture with a mass fraction of 30%, and after the reaction was completed, the mixture was slowly cooled to room temperature at a cooling rate of 2°C / min, filtered and washed to obtain a mixture D; S5: Mixture C and mixture D in a mass ratio of 3:1, add 3 wt % praseodymium oxide, and grind in a ball mill at a speed of 600 r / min for 2 h to obtain mixture E; S6: heating the polyvinyl alcohol to 85° C., stirring at a speed of 200 r / min, adding mixture E while stirring, wherein the mass ratio of mixture E to polyvinyl alcohol is 1:1, and then adding 1 wt % of polyethylene glycol 10000, stirring for 3 h, to obtain mixture F; S7: soaking the yarn in deionized water, heating to 100°C, reacting for 3 hours, taking out the yarn, and drying it at 110°C for 24 hours; S8: Use nitrogen to purge the dried yarn, the purge flow rate of nitrogen is 10m / s, and the purged yarn is immersed in mixture F for 8h at a temperature of 80°C. After the immersion is completed, the yarn is dried by a laser drying method. The parameters of the laser drying method are laser power 300W, temperature 60°C, and irradiation time 30min to obtain the photothermal conversion yarn.

[0031] Example 4 S1: Tungsten trioxide, zirconium carbide and carbon nanotubes were mixed in a mass ratio of 4:1:2, and ground in a ball mill at a speed of 500 r / min for 2 h to obtain a mixture A, wherein the particle size of the mixture A was 200 meshes; S2: dissolving graphene oxide in deionized water to obtain a graphene oxide solution with a mass fraction of 50%, dispersing mixture A in the graphene oxide solution, wherein the mass ratio of mixture A to graphene oxide is 1:2, and ultrasonicating for 1 h to obtain a solid-liquid mixture B; S3: The solid-liquid mixture after ultrasonication is placed in liquid nitrogen for freeze-drying for 15 minutes, and then dried at -50°C for 6 hours, and the solid obtained after freeze-drying is crushed and ground to obtain a mixture C, wherein the particle size of the mixture C is 200 mesh; S4: A 20% by mass hydrogen peroxide solution and a 20% by mass sulfuric acid solution were mixed in a volume ratio of 1:1 to obtain a mixed solution, silicon carbide was dispersed in the mixed solution, heated to 50°C, stirred at a speed of 150 r / min for 3 hours to obtain a solid-liquid mixture with a mass fraction of 30%, and after the reaction was completed, the mixture was slowly cooled to room temperature at a cooling rate of 2°C / min, filtered and washed to obtain a mixture D; S5: Mixture C and mixture D in a mass ratio of 3:1, add 3 wt % rubidium oxide, and grind in a ball mill at a speed of 600 r / min for 1 h to obtain mixture E; S6: heating the polyvinyl alcohol to 85° C., stirring at a speed of 200 r / min, adding mixture E while stirring, wherein the mass ratio of mixture E to polyvinyl alcohol is 1:1, and then adding 1 wt % of polyethylene glycol 5000, stirring for 3 h, to obtain mixture F; S7: soaking the yarn in deionized water, heating to 100°C, reacting for 3 hours, taking out the yarn, and drying it at 110°C for 24 hours; S8: Use nitrogen to purge the dried yarn, the purge flow rate of nitrogen is 8m / s, and the purged yarn is immersed in mixture F for 6h at a temperature of 80°C. After the immersion is completed, the yarn is dried by a laser drying method. The parameters of the laser drying method are laser power 300W, temperature 60°C, and irradiation time 30min to obtain the photothermal conversion yarn.

[0032] Comparative Example 1 In this comparative example, no tungsten trioxide was added during the preparation process, and the remaining steps were consistent with those of Example 1.

[0033] Comparative Example 2 In this comparative example, zirconium carbide is not added during the preparation process, and the remaining steps are consistent with those of Example 1.

[0034] Comparative Example 3 In this comparative example, no carbon nanotubes were added during the preparation process, and the remaining steps were consistent with those in Example 1.

[0035] Comparative Example 4 In this comparative example, steps S2 and S3 are not performed during the preparation process, and the remaining steps are consistent with those in Example 1.

[0036] Comparative Example 5 In this comparative example, silicon carbide was not added during the preparation process, and the remaining steps were consistent with those in Example 1.

[0037] Comparative Example 6 In this comparative example, no rare earth oxide is added during the preparation process, and the remaining steps are consistent with Example 1.

[0038] The embodiments and comparative examples were tested by using a spectrophotometer to test the absorbance and a thermal imager to test the photothermal conversion efficiency. The testing method is as follows: Taking sunlight as the light source, a spectroscope is used to split the light emitted by the light source into two beams of light, one of which is used to irradiate the yarn sample to be tested to heat the sample and a thermal imager is used to record the temperature change value of the sample. At the same time, the first optical power value of the other of the two beams of light is recorded, and the photothermal conversion efficiency of the sample is calculated based on the first optical power value and the temperature change value.

[0039] The experimental data are summarized in the following table:

[0040] Experimental data show that the addition of tungsten trioxide, zirconium carbide, carbon nanotubes, graphene oxide, silicon carbide and rare earth oxides effectively improves the performance of photothermal conversion yarn.

[0041] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a photothermal conversion yarn, It is characterized in that The preparation method of the photothermal conversion yarn is as follows: S1: tungsten trioxide, zirconium carbide and carbon nanotubes are mixed in a mass ratio of (3-5):1:2, and ground in a ball mill at a speed of 500 r / min for 1-2 h to obtain a mixture A; S2: dissolving graphene oxide in deionized water to obtain a graphene oxide solution with a mass fraction of 30-50%, dispersing mixture A in the graphene oxide solution, wherein the mass ratio of mixture A to graphene oxide is 1:(1-3), and ultrasonicating for 0.5-2h to obtain a solid-liquid mixture B; S3: freeze-dry the solid-liquid mixture after ultrasound in liquid nitrogen for 10-15 min, and then dry it at -50--30°C for 4-6 h, and grind the solid obtained after freeze-drying to obtain a mixture C; S4: A 20% by mass hydrogen peroxide solution and a 20% by mass sulfuric acid solution are mixed in a volume ratio of 1:1 to obtain a mixed solution, silicon carbide is dispersed in the mixed solution, heated to 50°C, stirred at a speed of 150 r / min for 2-3 hours to obtain a solid-liquid mixture with a mass fraction of 20-30%, and after the reaction is completed, slowly cooled to room temperature, filtered and washed to obtain a mixture D; S5: Mix the mixture C and the mixture D in a mass ratio of (1-3):1, add 2-3 wt% of rare earth oxide, and grind in a ball mill at a speed of 500-600 r / min for 1-2 h to obtain a mixture E; S6: heating the polyvinyl alcohol to 75-85° C., stirring at a speed of 200 r / min, adding mixture E while stirring, wherein the mass ratio of mixture E to polyvinyl alcohol is 1:1, and then adding 0.5-1wt% of a dispersant, stirring for 2-3 h, to obtain mixture F; S7: soaking the yarn in deionized water, heating to 100°C, reacting for 2-3 hours, taking out the yarn, and drying it at 110°C for 24 hours; S8: Use nitrogen to purge the dried yarn, and immerse the purged yarn in the mixture F for 6 to 8 hours at a temperature of 80°C. After the immersion is completed, use a laser drying method to dry the yarn to obtain the photothermal conversion yarn.

2. A method for preparing a photothermal conversion yarn according to claim 1, It is characterized in that The particle size of the mixture A in S1 is 200 mesh.

3. The method for preparing a photothermal conversion yarn according to claim 1, It is characterized in that The particle size of the mixture C in S3 is 200 mesh.

4. The method for preparing a photothermal conversion yarn according to claim 1, It is characterized in that The cooling rate in S4 is 2°C / min.

5. The method for preparing a photothermal conversion yarn according to claim 1, It is characterized in that The rare earth oxide in S5 is one or more of cerium oxide, lanthanum oxide, praseodymium oxide and rubidium oxide.

6. A method for preparing a photothermal conversion yarn according to claim 1, It is characterized in that The dispersant in S6 is polyethylene glycol, and its number average molecular weight is 2000-10000.

7. A method for preparing a photothermal conversion yarn according to claim 1, It is characterized in that The purge flow rate of nitrogen in S8 is 8-10 m / s.

8. The method for preparing a photothermal conversion yarn according to claim 1, It is characterized in that The parameters of the laser drying method in S8 are: laser power 300 W, temperature 60° C., and irradiation time 30 min.

Citation Information

Cited By

  • Thermal insulation material as well as preparation method and application thereof

    CN120331041A