Spinning oil agent special for hollow fibers and preparation method of spinning oil agent

By using a combination of emulsifier, silicone oil, smoothing agent and antistatic agent on the hollow fiber, the problem of fiber vulnerability is solved, the fiber abutment and anti-friction performance is improved, the fiber is protected from damage, and the fiber is better Fiber protection effect.

CN119041209APending Publication Date: 2024-11-29TONGXIANG HENGLONG CHEM CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411119357.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Due to its specific structure, hollow fibers are easily damaged when subjected to external forces. A spinning oil agent with excellent performance is urgently needed to improve the abutment of the fibers and reduce friction, protect the fibers from damage.

Method used

Using a special spinning oil agent for hollow fibers, including emulsifiers, silicone oils, smoothing agents, and antistatic agents, by selecting appropriate fatty alcohol polyoxyethylene polyoxypropylene ether as the smoothing agent, combined with modified penetration agent and highly reactive phosphoric acid Ester, enhances the strength of the oil film, and uses quaternary ammonium salt to reduce fiber surface resistance, reducing electrostatic accumulation and friction.

Benefits of technology

It effectively improves the abutment of fibers, reduces fiber friction and wire breakage, enhances the permeability and dispersion of oil agents, and protects the fiber from damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0004994577340000011
    Figure FDA0004994577340000011
Patent Text Reader

Abstract

The invention discloses a spinning oil agent special for hollow fibers and a preparation method thereof. The spinning oil agent comprises the following components in parts by weight: 45-58 parts of an emulsifier; 0.02 to 0.04 part of silicone oil; 1-2 parts of a modified penetrant; 0.01 to 0.05 part of a smoothing agent; and 3-5 parts of an antistatic agent. The antistatic agent is any one or more of fatty alcohol-polyoxyethylene ether potassium salt, quaternary ammonium salt and fatty alcohol-polyoxyethylene ether phosphate potassium salt. The spinning oil agent special for the hollow fibers has good oil film strength, so that the cohesion of the fibers is improved, the friction of the fibers is reduced, and the fibers can be better protected from being damaged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fiber oils, and in particular to a special spinning oil for hollow fibers and a preparation method thereof. Background Art

[0002] Hollow fiber is a polymer fiber with a special structure, which is widely used in textile, packaging, medical and other fields. Compared with ordinary fibers, hollow fiber has better warmth retention, air permeability and moisture absorption, so it is widely used in making high-end thermal underwear, socks, outdoor clothing, etc. At the same time, hollow fiber can also be used to make medical materials.

[0003] Chinese patent CN1314507A hollow fiber and hollow fiber manufacturing method, the invention provides hollow fiber and fiber structure containing the fiber, which is composed of a polymer that does not show water absorption and has excellent porous hollow parts such as light weight, dry feeling, and fluffy feeling. The fiber structure of sea-island type composite fiber containing a thermoplastic polymer with an equilibrium moisture content of less than 2% as a sea component and a water-soluble thermoplastic polyvinyl alcohol polymer as an island component is treated with water, and at least a part of the water-soluble thermoplastic polyvinyl alcohol polymer is dissolved and removed from the composite fiber.

[0004] However, due to its specific structure, the hollow fiber is easily damaged when it receives external force, thereby causing damage to the fiber.

[0005] In summary, there is an urgent need for a special spinning oil for hollow fibers with excellent performance. The special spinning oil for hollow fibers should have good oil film strength to improve the cohesion of the fibers and reduce fiber friction, thereby better protecting the fibers from damage. Summary of the invention

[0006] The technical problems to be solved by the present invention are:

[0007] A special spinning oil for hollow fibers and a preparation method thereof are developed. The special spinning oil for hollow fibers has good oil film strength to improve the cohesion of the fibers and reduce fiber friction, thereby better protecting the fibers from damage.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] A spinning oil for hollow fibers, comprising the following components in parts by weight:

[0010] Emulsifier: 45-58 parts;

[0011] Silicone oil: 0.02-0.04 parts;

[0012] Smoothing agent: 0.01~0.05 parts

[0013] Antistatic agent: 3 to 5 parts.

[0014] As a further improvement of this solution, the antistatic agent is any one or more of fatty alcohol polyoxyethylene ether potassium salt, quaternary ammonium salt, and fatty alcohol polyoxyethylene ether phosphate potassium salt.

[0015] As a further improvement of this solution, the antistatic agent is a quaternary ammonium salt.

[0016] As a further improvement of this solution, the lubricant is fatty alcohol polyoxyethylene polyoxypropylene ether.

[0017] As a further improvement of this solution, the molecular weight of the fatty alcohol polyoxyethylene polyoxypropylene ether is 4000.

[0018] As a further improvement of this solution, the modified penetrant includes

[0019] 15-18 parts of polyoxyethylene polyoxypropylene ether;

[0020] 40-50 parts of lubricating oil;

[0021] Emulsifier 4-5 parts

[0022] 0.1 to 0.5 parts of bimetallic catalyst.

[0023] As a further improvement of this solution, the emulsifier is: 1 to 2 parts of dodecanol polyoxyethylene polyoxypropylene;

[0024] 4-8 parts of propylene glycol random polyether;

[0025] 3-6 parts of isomeric decanol polyoxyethylene ether

[0026] 2 to 4 parts of isomeric alcohol ether mixture.

[0027] As a further improvement of this solution, the bimetallic catalyst is a bimetallic cyanide complex DMC.

[0028] As a further improvement of this solution, the raw materials of the following components are mixed and stirred:

[0029] Emulsifier: 45-58 parts;

[0030] Silicone oil: 0.02-0.04 parts;

[0031] Modified penetrant: 1-2 parts;

[0032] Smoothing agent: 0.01~0.05 parts

[0033] Antistatic agent: 3 to 5 parts.

[0034] Finally, a special spinning oil for hollow fibers is obtained;

[0035] The modified penetrant is prepared according to the following steps: 15 to 18 parts of polyoxyethylene polyoxypropylene ether and 40 to 50 parts of lubricating oil are stirred and mixed, and then 4 to 5 parts of emulsifier are added. During the stirring process, a bimetallic catalyst is added, and the reaction temperature is 35 to 45° C. and stirred for 8 to 12 hours.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] 1) Selection and proportion of lubricant: Fatty alcohol polyoxyethylene polyoxypropylene ether is selected as the lubricant, and the molecular weight is controlled at 4000; furthermore, by cooperating with the modified penetrant and the lubricant, the oil film strength can be enhanced, the fiber adhesion can be improved, the fiber friction can be reduced, and the hollow fiber can be better protected from damage.

[0038] 2) Adding quaternary ammonium salt as antistatic agent: Adding quaternary ammonium salt at a ratio of 5% can effectively reduce the surface resistance of the fiber and prevent static electricity accumulation. It can also reduce the friction between fibers and between fibers and devices, and effectively reduce broken fibers.

[0039] 3) Adding highly active phosphate LYCO-P08: Adding 0.5-1.0% of highly active phosphate LYCO-P08 can increase the dispersibility and solubility of the oil and enhance the penetration performance of the oil. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention is further described below in conjunction with embodiments:

[0041] Example 1

[0042] A spinning oil for hollow fibers, comprising the following components in parts by weight:

[0043] Emulsifier: 50 parts;

[0044] Silicone oil: 0.03 parts;

[0045] Modified penetrant: 2 parts;

[0046] Smoothing agent: 0.04 parts

[0047] Antistatic agent: 4 parts.

[0048] The antistatic agent is a quaternary ammonium salt.

[0049] The lubricant is fatty alcohol polyoxyethylene polyoxypropylene ether.

[0050] The molecular weight of fatty alcohol polyoxyethylene polyoxypropylene ether is 4000.

[0051] Modified penetrants include

[0052] 16 parts of polyoxyethylene polyoxypropylene ether;

[0053] 45 parts of lubricating oil;

[0054] Emulsifier 5 parts

[0055] 0.3 parts of bimetallic catalyst.

[0056] The emulsifier is a mixture of the following components: 1 part of polyoxyethylene polyoxypropylene of dodecanol; 6 parts of propylene glycol random polyether; 4 parts of isomeric decanol polyoxyethylene ether; and 3 parts of isomeric alcohol ether mixture.

[0057] In this embodiment, the modified penetrant in the hollow fiber special spinning oil is prepared according to the following preparation steps:

[0058] The polyoxyethylene polyoxypropylene ether and lubricating oil are stirred and mixed, and then an emulsifier is added. During the stirring process, a bimetallic catalyst is added. The reaction temperature is 35 to 45° C. and the stirring is performed for 8 to 12 hours. The final reaction product is a spinning oil agent specifically for hollow fibers.

[0059] Preparation of hollow fiber spinning oil

[0060] The raw materials of each component are accurately prepared, added into a reaction kettle, heated to 40°C, stirred for 1-3 minutes, and cooled to room temperature; finally, filtered, discharged and packaged to obtain a special spinning oil for hollow fibers.

[0061] Comparative Example 1

[0062] The formula components in the comparative example are consistent with those in Example 1.

[0063] The only difference is that there is no modified penetrant.

[0064] Comparative Example 2

[0065] The formula components in the comparative example are basically the same as those in Example 1.

[0066] The only difference is that the penetrant is commercially available.

[0067] The test results of the special spinning oil for hollow fibers in Example 1 are shown in Table 1 below:

[0068] Table 1 Test results of hollow fiber special spinning oil

[0069] Test items Standard requirements Test results Single judgment 1 Appearance (25℃) Yellow transparent liquid Yellow transparent liquid conform to 2 pH (1% aqueous solution) 6.5~9.5 8.2 conform to 3 Conductivity (10% aqueous solution), μS / cm ≥400 616 conform to 4 Effective content, % 86~91 88 conform to 5 <![CDATA[Kinematic viscosity (40 °C), mm 2 / s]]> 70~120 92 conform to

[0070] Table 2 Test results of Example 1 and Comparative Examples 1-2

[0071] Test items Example 1 Comparative Example 1 Comparative Example 2 Broken wire 0.8 times / line*day 8-10 times / line*day 5.6 times / line*day

[0072] The special spinning oil for hollow fibers in Example 1 and Comparative Examples 1 to 3 were tried to investigate the fiber breakage situation.

[0073] Selecting fatty alcohol polyoxyethylene polyoxypropylene ether as a lubricant and combining it with a modified penetrant, while controlling the molecular weight reduction to 4000, can enhance the oil film strength, improve the fiber's cohesion, reduce fiber friction, and better protect the fiber from damage. Adding quaternary ammonium salt as an antistatic agent: adding 5% quaternary ammonium salt can effectively reduce the surface resistance of the fiber and prevent static electricity accumulation. Reduce the friction between fibers and between fibers and porcelain parts, and reduce broken wires. Adding highly active phosphate LYCO-P08 and improving the penetrant: adding 0.5-1.0% of highly active phosphate LYCO-P08 can increase the dispersibility and solubility of FDY oil and enhance the penetration performance of the oil.

[0074] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent changes made using the present invention are within the patent protection scope of the present invention.

Claims

1. A spinning oil for hollow fibers, characterized in that: The composition comprises the following components in parts by weight: Emulsifier: 45-58 parts; Silicone oil: 0.02-0.04 parts; Modified penetrant: 1-2 parts; Smoothing agent: 0.01-0.05 parts; Antistatic agent: 3 to 5 parts.

2. The hollow fiber spinning oil according to claim 1, characterized in that: The antistatic agent is any one or more of fatty alcohol polyoxyethylene ether potassium salt, quaternary ammonium salt, and fatty alcohol polyoxyethylene ether phosphate potassium salt.

3. The hollow fiber spinning oil according to claim 3, characterized in that: The antistatic agent is a quaternary ammonium salt.

4. The hollow fiber spinning oil according to claim 1, characterized in that: The lubricant is fatty alcohol polyoxyethylene polyoxypropylene ether.

5. The hollow fiber spinning oil according to claim 4, characterized in that: The molecular weight of fatty alcohol polyoxyethylene polyoxypropylene ether is 4000.

6. The hollow fiber spinning oil according to claim 1, characterized in that: Modified penetrants include 7. The hollow fiber spinning oil according to claim 6, characterized in that the emulsifier is: 1 to 2 parts of polyoxyethylene polyoxypropylene of dodecanol; 4-8 parts of propylene glycol random polyether; 3-6 parts of isomeric decanol polyoxyethylene ether 2 to 4 parts of isomeric alcohol ether mixture.

8. The hollow fiber spinning oil according to claim 6, characterized in that: The bimetallic catalyst is a double metal cyanide complex DMC.

9. The hollow fiber spinning oil according to claim 6, characterized in that: The hollow fiber spinning oil is prepared according to the following steps: Mix and stir the following raw materials: Emulsifier: 45-58 parts; Silicone oil: 0.02-0.04 parts; Modified penetrant: 1-2 parts; Smoothing agent: 0.01~0.05 parts Antistatic agent: 3 to 5 parts. Finally, a special spinning oil for hollow fibers is obtained; The modified penetrant is prepared according to the following steps: 15 to 18 parts of polyoxyethylene polyoxypropylene ether and 40 to 50 parts of lubricating oil are stirred and mixed, and then 4 to 5 parts of emulsifier are added, and a bimetallic catalyst is added during the stirring process. The reaction temperature is 35 to 45° C. and stirred for 8 to 12 hours.

Citation Information

Patent Citations

  • Hollow fibre and method for producing hollow fibre

    CN1314507A