Novel white gold paper for gold foil forging and preparation method of novel white gold paper

By using temperature-resistant coating and specific process treatment on Wujin paper, the tensile strength and gold foil yield of Wujin paper are improved, and the problems of insufficient tensile strength and high gold consumption of traditional Wujin paper are solved, thus achieving more efficient Gold foil forging process.

CN119041244APending Publication Date: 2024-11-29NANJING GOLD LINE & GOLD FOIL FACTORY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411177057.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing new black gold paper for forging of gold foil has insufficient tensile strength, many sand holes, serious splicing, and high gold consumption.

Method used

The temperature-resistant coating consists of silicon oxide, silicon carbide, silicone resin, monoglyceride stearic acid, myristyl alcohol and ultrapure water. The black gold paper is prepared by dipping paper, drying, ink coating, stamping and cutting processes. , improve its tensile strength and utilization rate.

Benefits of technology

It significantly improves the tensile strength and gold foil yield of black gold paper, reduces the gold foil consumption, extends the service life and increases the foil extension speed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119041244A_ABST
    Figure CN119041244A_ABST
Patent Text Reader

Abstract

The invention discloses novel white gold paper for gold foil forging and a preparation method thereof, and relates to the technical field of white gold paper, and the preparation method comprises the following steps: step s1, carrying out paper immersion and drying on yellow paper a to form yellow paper b, step s2, coating the surface of the yellow paper b with ink to form yellow paper c, step s3, coating the surface of the yellow paper c with a surface temperature-resistant coating to form yellow paper d, and step s4, carrying out drying to form the novel white gold paper for gold foil forging. The manufacturing method comprises the following steps of S1, placing yellow paper d into a drying box to be dried to form a base material a, S2, stamping the base material a to extend the base material a to form a base material b, and S3, cutting the base material b to obtain the white gold paper. The temperature-resistant coating comprises the following temperature-resistant coating raw materials in parts by weight: 20-35 parts of silicon oxide, 15-35 parts of silicon carbide, 13-24 parts of organic silicon resin, 4-6 parts of glycerol monostearate, 2-5 parts of oleayl, 3-9 parts of myristyl alcohol, 2-8 parts of diethylenetriamine and 65-132 parts of ultrapure water, the temperature-resistant coating raw materials are formed by mixing and stirring, and the temperature-resistant coating raw materials are mixed through a reaction kettle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of black gold paper, in particular to a new type of black gold paper used for gold foil forging and a preparation method thereof. Background Art

[0002] The application areas of gold foil and its products have gradually developed from simple gilding of ancient buildings to medicine, handicrafts, cosmetics, food, furniture and modern architecture. Due to the expansion of the application scope, users have higher requirements for the quality of gold foil. The original traditional production process technology has not kept up with the development of the times. Therefore, it is necessary to improve product quality, upgrade product grade, increase labor productivity, reduce costs and increase efficiency. However, a crucial factor affecting product quality is the production level of black gold paper, the carrier material used for hammering gold foil. It has many sand holes, serious splicing and high gold consumption.

[0003] The defects of the new black gold paper used for forging gold foil are:

[0004] 1. Patent document CN101446056B discloses a method for manufacturing black gold paper and a special black smoke glue for manufacturing black gold paper and a preparation method thereof. "According to the disclosed black smoke glue formula, first add measured borax, ammonia water, and casein to water and stir to dissolve, then add measured high-pigment carbon black and other chemical raw materials, and then add water to ensure that the solid content in the mixed substance is 12%-18% of the total weight, and then grind evenly, filter out impurities, and obtain the black smoke glue for coating the surface of black gold paper. Then, glassine paper or translucent paper is used as the original blank paper, and special black smoke glue is coated on both sides to prepare black gold paper. The method for preparing black gold paper of the present invention has few steps, high efficiency, short production cycle, high yield, low labor intensity, excellent quality, fast extension speed of producing hammered gold foil, good uniformity of gold foil, flatness, brightness, no sand holes, low gold consumption, etc." However, compared with traditional paper, the existing new black gold paper for forging gold foil has no obvious improvement in tensile strength, many sand holes, serious splicing, and high gold consumption;

[0005] 2. Patent document CN217867303U discloses an automatic black gold paper edge adjustment production system, "including a PLC control box and a transmission device, a vacuum adsorption device and a feeding device electrically connected to the controller in the PLC control box through cables, the transmission device includes a lifting cylinder, a placement slot module, a suction cup, a metal bracket and a screw servo motor; a screw servo motor is arranged on the panel of the metal bracket, a fixed plate is arranged on the slider on the screw of the screw servo motor, a lifting cylinder is installed on both sides, a fixed block is arranged at the bottom of the telescopic rod of each lifting cylinder, a connecting plate is arranged at the bottom of the fixing block, an I-shaped bracket is installed on both sides, and each I-shaped bracket has four corners with holes and air nozzles, and is connected to the vacuum adsorption device through an air pipe, and a placement slot module is arranged on the left and right sides of the metal bracket, and a feeding device is arranged at the bottom; the utility model solves the problem of black gold paper stacking caused by distraction in manual assembly line production", but the existing new black gold paper used for gold foil forging has a low gold foil yield rate compared with traditional paper;

[0006] 3. Patent document CN215152427U discloses an automatic pressing device for gold foil made of black gold paper, "including a frame, a lifting device and a pressure sensor, the frame includes an upper support plate, a middle support plate, a bottom plate and a column, the four corners of the bottom plate are provided with columns, the upper ends of the four columns respectively pass through the fixed holes set at the four corners of the middle support plate, and the tops thereof are fixedly connected with the four corners of the upper support plate by screws, the lifting device is installed on the upper support plate, the driving motor is connected to the reducer 1, the reducer 1 is connected to the reducer 2, the lifting shaft of the lift passes through the through hole set on the upper support plate, the bottom of which is fixedly connected with a pressing block, the middle support plate is provided with a pressing platform used in conjunction with the pressing plate, and a pressure sensor is provided at the bottom of the pressing platform; the utility model has a high degree of automation, can reduce the labor intensity of workers and improve the safety of workers, and at the same time can freely adjust the size of the pressure, and can accurately achieve the ideal pressing effect", but compared with the traditional paper, the utilization rate of the existing new black gold paper used for gold foil forging is not high;

[0007] 4. Patent document CN112139440B discloses a assembling machine and its use method, "including a frame, a cutting mechanism, an assembly table, a mechanical arm and a core controller, a baffle is fixedly connected to the top of the inner wall of the black gold paper box, an assembly table, the assembly table includes a black gold paper box and an assembly box, and an air nozzle is provided on the top of the inner wall of the black gold paper box, and the baffle and the air nozzle can separate the bonded black gold paper. The present invention can continuously and automatically cut out metal sheets through the cutting mechanism, and through the setting of the mechanical arm, a layer of black gold paper can be placed from the black gold paper box into the assembly box first, and then a piece of metal sheet can be placed on the black gold paper in the assembly box, and the cycle is carried out in sequence, thereby improving the efficiency of assembling metal sheets and black gold paper, and the operation is stable and the assembly accuracy is high. Through the coordinated use of the baffle and the air nozzle, the bonded black gold paper can be separated, which further improves the assembly efficiency. The present invention has a simple and reasonable structural design, is convenient and quick to use, and has strong practicality", but the existing new black gold paper used for gold foil forging consumes a large amount of gold foil compared with traditional paper. Summary of the invention

[0008] The purpose of the present invention is to provide a new type of black gold paper for gold foil forging and a preparation method thereof, so as to solve the technical problems proposed in the above background technology that the existing new type of black gold paper for gold foil forging has no obvious improvement in tensile strength compared with traditional paper, has many sand holes, serious splicing, and high gold consumption.

[0009] To achieve the above object, the present invention provides the following technical solution: a method for preparing a new type of black gold paper for gold foil forging, comprising the following steps:

[0010] Step s1, soaking and drying yellow paper a to form yellow paper b:

[0011] Step s2, applying ink on the surface of yellow paper b to form yellow paper c:

[0012] Step s3, coating the surface of yellow paper c with a temperature-resistant coating to form yellow paper d;

[0013] Step s4, placing the yellow paper d into a drying box for drying to form a substrate a:

[0014] Step s5, punching the substrate a to extend it to form a substrate b:

[0015] Step s6, cutting the substrate b to obtain black gold paper;

[0016] The heat-resistant coating comprises the following raw materials of the heat-resistant coating in parts by weight: 20 to 35 parts of silicon oxide, 15 to 35 parts of silicon carbide, 13 to 24 parts of silicone resin, 4 to 6 parts of stearic acid monoglyceride, 2 to 5 parts of oleic acid, 3 to 9 parts of myristyl alcohol, 2 to 8 parts of diethylenetriamine and 65 to 132 parts of ultrapure water. The raw materials of the heat-resistant coating are formed by mixing and stirring. The raw materials of the heat-resistant coating are mixed in a reactor. Before mixing, the raw materials of the heat-resistant coating are filtered for impurities through a 20 to 40 mesh filter screen. The mixing time of the raw materials of the heat-resistant coating is 1 to 1.8 hours, and the temperature of the raw materials of the heat-resistant coating when mixed is 25 to 45°C.

[0017] Preferably, the yellow paper a is made of young bamboo.

[0018] Preferably, the ink includes bituminous coal and water. The bituminous coal is smoked on a smoke collecting vessel generated by coal combustion. The quality of the bituminous coal is improved by adjusting the combustion temperature of the coal. After smoking, the bituminous coal is scraped off the collecting vessel. The bituminous coal is washed and filtered to remove impurities and excess water.

[0019] Preferably, the ink also includes an epoxy resin adhesive, which has epoxy and reaction activity and can form strong adhesion after cross-linking polymerization.

[0020] Preferably, the ink also includes a coupling agent and a cross-linking agent, which couple the epoxy resin adhesive in the ink with the polymer printing material to form a coupling body, thereby improving the fixing effect of the ink, and reducing the film-forming temperature of the adhesive, thereby improving the adhesion of the ink. The ink is cured by the power of a UV light curing lamp, and the curing wavelength of the UV lamp can be adjusted according to the different inks to achieve a better curing effect.

[0021] Preferably, during the production process of the yellow paper b, the drying temperature of the yellow paper b is 60-80° C., the drying time of the yellow paper b is 10-30 minutes, and the humidity of the dried yellow paper b is maintained at 15-25%.

[0022] Preferably, the ink is applied on the surface of the yellow paper b to a thickness of 0.2 mm to 0.4 mm.

[0023] Preferably, the yellow paper b is dyed and waxed, and the yellow paper b is dyed by using a Phellodendron chinense extract, and the Phellodendron chinense extract increases the folding strength of the yellow paper b.

[0024] Preferably, the yellow paper b is coated with yellow wax, and the yellow wax makes the paper smooth and firm.

[0025] Preferably, the black gold paper is made by the preparation method of the novel black gold paper.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1. The present invention is provided with a heat-resistant coating comprising the following weight parts of heat-resistant coating raw materials: 22 parts of silicon oxide, 18 parts of silicon carbide, 15 parts of silicone resin, 5 parts of stearic acid monoglyceride, 2 parts of oleic acid, 4 parts of myristyl alcohol, 2 parts of diethylenetriamine, and 70 parts of ultrapure water. The heat-resistant coating raw materials are formed by mixing and stirring. The heat-resistant coating raw materials are mixed by a reactor. The heat-resistant coating raw materials are filtered through a 25-mesh filter screen before mixing. The mixing time of the heat-resistant coating raw materials is 1 hour. The temperature of the heat-resistant coating raw materials when mixed is 30°C. The yellow paper a is made of young bamboo. The ink comprises bituminous coal and water. The bituminous coal is smoked on a smoke collecting vessel generated by coal combustion. The bituminous coal improves its quality by adjusting the combustion temperature of the coal. After smoking, the bituminous coal is scraped off the collecting vessel. Compared with traditional paper, the tensile strength of the black gold paper is significantly improved, the service life is increased by 1-3 times, and the foil extension speed is increased by more than one time.

[0028] 2. The present invention is provided with a heat-resistant coating comprising the following weight parts of heat-resistant coating raw materials: 22 parts of silicon oxide, 18 parts of silicon carbide, 15 parts of silicone resin, 5 parts of stearic acid monoglyceride, 2 parts of oleic acid, 4 parts of myristyl alcohol, 2 parts of diethylenetriamine, and 70 parts of ultrapure water. The heat-resistant coating raw materials are formed by mixing and stirring. The heat-resistant coating raw materials are mixed by a reactor. The heat-resistant coating raw materials are filtered through a 25-mesh filter screen before mixing. The mixing time of the heat-resistant coating raw materials is 1 hour. The temperature of the heat-resistant coating raw materials when mixed is 30°C. The yellow paper a is made of young bamboo. The ink comprises bituminous coal and water. The bituminous coal is smoked on a smoke collecting vessel generated by coal combustion. The bituminous coal improves its quality by adjusting the combustion temperature of the coal. After smoking, the bituminous coal is scraped off the collecting vessel, so that the gold foil yield rate of the black gold paper is significantly improved compared with traditional paper.

[0029] 3. The present invention is provided with a heat-resistant coating comprising the following weight parts of heat-resistant coating raw materials: 22 parts of silicon oxide, 18 parts of silicon carbide, 15 parts of silicone resin, 5 parts of stearic acid monoglyceride, 2 parts of oleic acid, 4 parts of myristyl alcohol, 2 parts of diethylenetriamine, and 70 parts of ultrapure water. The heat-resistant coating raw materials are formed by mixing and stirring. The heat-resistant coating raw materials are mixed by a reactor. The heat-resistant coating raw materials are filtered through a 25-mesh filter screen before mixing. The mixing time of the heat-resistant coating raw materials is 1 hour. The temperature of the heat-resistant coating raw materials when mixed is 30°C. The yellow paper a is made of young bamboo. The ink comprises bituminous coal and water. The bituminous coal is smoked on a smoke collecting vessel generated by coal combustion. The bituminous coal improves its quality by adjusting the combustion temperature of the coal. After smoking, the bituminous coal is scraped off the collecting vessel, thereby achieving a significant improvement in the utilization rate of the black gold paper compared with traditional paper.

[0030] 4. The present invention is provided with a heat-resistant coating comprising the following heat-resistant coating raw materials in parts by weight: 22 parts of silicon oxide, 18 parts of silicon carbide, 15 parts of silicone resin, 5 parts of stearic acid monoglyceride, 2 parts of oleic acid, 4 parts of myristyl alcohol, 2 parts of diethylenetriamine, and 70 parts of ultrapure water. The heat-resistant coating raw materials are formed by mixing and stirring. The heat-resistant coating raw materials are mixed through a reactor. The heat-resistant coating raw materials are filtered for impurities through a 25-mesh filter before mixing. The mixing time of the heat-resistant coating raw materials is 1 hour. The temperature of the heat-resistant coating raw materials when mixed is 30°C. The yellow paper a is made of young bamboo. The ink comprises bituminous coal and water. The bituminous coal is smoked on a smoke collecting vessel generated by coal combustion. The bituminous coal quality is improved by adjusting the combustion temperature of the coal. After smoking, the bituminous coal is scraped off the collecting vessel, thereby achieving a significant reduction in the gold foil consumption compared with traditional paper. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a schematic diagram of experimental data of the present invention. DETAILED DESCRIPTION

[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] In the description of the present invention, it should be noted that the terms "upper", "lower", "inner", "outer", "front end", "rear end", "two ends", "one end", "the other end" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0034] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "provided with", "connected", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, it can be understood according to the specific situation.

[0035] Embodiment 1: An embodiment provided by the present invention: A method for preparing a new type of black gold paper for gold foil forging, comprising the following steps:

[0036] Step s1, soaking and drying yellow paper a to form yellow paper b:

[0037] Step s2, applying ink on the surface of yellow paper b to form yellow paper c:

[0038] Step s3, coating the surface of yellow paper c with a temperature-resistant coating to form yellow paper d;

[0039] Step s4, placing the yellow paper d into a drying box for drying to form a substrate a:

[0040] Step s5, punching the substrate a to extend it to form a substrate b:

[0041] Step s6, cutting the substrate b to obtain black gold paper;

[0042] The heat-resistant coating comprises the following parts by weight of heat-resistant coating raw materials: 22 parts of silicon oxide, 18 parts of silicon carbide, 15 parts of silicone resin, 5 parts of stearic acid monoglyceride, 2 parts of oleic acid, 4 parts of myristyl alcohol, 2 parts of diethylenetriamine, and 70 parts of ultrapure water. The heat-resistant coating raw materials are formed by mixing and stirring. The heat-resistant coating raw materials are mixed in a reactor. The heat-resistant coating raw materials are filtered through a 25-mesh filter before mixing. The mixing time of the heat-resistant coating raw materials is 1 hour. The temperature of the heat-resistant coating raw materials when mixed is 30°C. The yellow paper a is made of young bamboo. The ink comprises bituminous coal and water. The bituminous coal is smoked on a smoke collection vessel generated by coal combustion. The quality of the bituminous coal is improved by adjusting the combustion temperature of the coal. After smoking, the bituminous coal is scraped off the collection vessel. The bituminous coal is washed and filtered to remove impurities and excess water. The ink also comprises an epoxy resin adhesive. The epoxy resin adhesive has epoxy and reaction activity and can form strong adhesion after cross-linking polymerization. The ink also includes a coupling agent and a cross-linking agent. The coupling agent and the cross-linking agent make the epoxy resin adhesive in the ink produce a coupling body with the polymer printing material, thereby improving the fixing effect of the ink, reducing the film-forming temperature of the adhesive, and improving the adhesion of the ink. The ink is cured by the power of a UV light curing lamp. The curing wavelength of the UV lamp can be adjusted according to the different inks to achieve a better curing effect. During the production process of the yellow paper b, the drying temperature of the yellow paper b is 60 to 80°C, the drying time of the yellow paper b is 10 to 30 minutes, and the humidity of the dried yellow paper b is maintained at 15 to 25%. The thickness of the ink applied on the surface of the yellow paper b is 0.2 mm to 0.4 mm. The yellow paper b is dyed and waxed. The yellow paper b is dyed by a coptis extract. The coptis extract increases the folding strength of the yellow paper b. The yellow paper b is coated with yellow wax. The yellow wax makes the paper smooth and firm. The black gold paper is made by the preparation method of the novel black gold paper.

[0043] Embodiment 2: An embodiment provided by the present invention: A method for preparing a new type of black gold paper for gold foil forging, comprising the following steps:

[0044] Step s1, soaking and drying yellow paper a to form yellow paper b:

[0045] Step s2, applying ink on the surface of yellow paper b to form yellow paper c:

[0046] Step s3, coating the surface of yellow paper c with a temperature-resistant coating to form yellow paper d;

[0047] Step s4, placing the yellow paper d into a drying box for drying to form a substrate a:

[0048] Step s5, punching the substrate a to extend it to form a substrate b:

[0049] Step s6, cutting the substrate b to obtain black gold paper;

[0050] The heat-resistant coating comprises the following parts by weight of heat-resistant coating raw materials: 29 parts of silicon oxide, 32 parts of silicon carbide, 21 parts of silicone resin, 5 parts of stearic acid monoglyceride, 4 parts of oleic acid, 6 parts of myristyl alcohol, 6 parts of diethylenetriamine, and 90 parts of ultrapure water. The heat-resistant coating raw materials are formed by mixing and stirring. The heat-resistant coating raw materials are mixed in a reactor. The heat-resistant coating raw materials are filtered through a 20-40 mesh filter before mixing. The mixing time of the heat-resistant coating raw materials is 1.1 hours. The temperature of the heat-resistant coating raw materials when mixed is 40°C. The yellow paper a is made of young bamboo. The ink comprises bituminous coal and water. The bituminous coal is smoked on a smoke collection vessel generated by coal combustion. The bituminous coal improves its quality by adjusting the combustion temperature of the coal. After smoking, the bituminous coal is scraped off the collection vessel. The bituminous coal is washed and filtered to remove impurities and excess water. The ink also comprises an epoxy resin adhesive. The epoxy resin adhesive has epoxy and reaction activity and can form strong adhesion after cross-linking polymerization. The ink also includes a coupling agent and a cross-linking agent, which allow the epoxy resin adhesive in the ink to produce a coupling body with the polymer printing material, thereby improving the fixing effect of the ink, reducing the film-forming temperature of the adhesive, and improving the adhesion of the ink. The ink is cured by the power of a UV light curing lamp, and the curing wavelength of the UV lamp can be adjusted according to the different inks to achieve a better curing effect. During the production process of the yellow paper b, the drying temperature of the yellow paper b is 60 to 80°C, the drying time of the yellow paper b is 10 to 30 minutes, and the humidity of the dried yellow paper b is maintained at 15 to 25%. The thickness of the ink applied on the surface of the yellow paper b is 0.2 mm to 0.4 mm. The yellow paper b is dyed and waxed, and the yellow paper b is dyed with a coptis extract, and the coptis extract increases the folding strength of the yellow paper b. The yellow paper b is coated with yellow wax, and the yellow wax makes the paper smooth and firm. The black gold paper prepared by the preparation method of the novel black gold paper.

[0051] Embodiment 3: An embodiment provided by the present invention: A method for preparing a new type of black gold paper for gold foil forging, comprising the following steps:

[0052] Step s1, soaking and drying yellow paper a to form yellow paper b:

[0053] Step s2, applying ink on the surface of yellow paper b to form yellow paper c:

[0054] Step s3, coating the surface of yellow paper c with a temperature-resistant coating to form yellow paper d;

[0055] Step s4, placing the yellow paper d into a drying box for drying to form a substrate a:

[0056] Step s5, punching the substrate a to extend it to form a substrate b:

[0057] Step s6, cutting the substrate b to obtain black gold paper;

[0058] The heat-resistant coating comprises the following parts by weight of heat-resistant coating raw materials: 28 parts of silicon oxide, 32 parts of silicon carbide, 20 parts of silicone resin, 4 parts of stearic acid monoglyceride, 3 parts of oleic acid, 7 parts of myristyl alcohol, 7 parts of diethylenetriamine, and 120 parts of ultrapure water. The heat-resistant coating raw materials are formed by mixing and stirring. The heat-resistant coating raw materials are mixed in a reactor. The heat-resistant coating raw materials are filtered through a 28-mesh filter before mixing. The mixing time of the heat-resistant coating raw materials is 1.6 hours. The temperature of the heat-resistant coating raw materials when mixed is 28°C. The yellow paper a is made of young bamboo. The ink comprises bituminous coal and water. The bituminous coal is smoked on a smoke collection vessel generated by coal combustion. The quality of the bituminous coal is improved by adjusting the combustion temperature of the coal. After smoking, the bituminous coal is scraped off the collection vessel. The bituminous coal is washed and filtered to remove impurities and excess water. The ink also comprises an epoxy resin adhesive. The epoxy resin adhesive has epoxy and reaction activity and can form strong adhesion after cross-linking polymerization. The ink also includes a coupling agent and a cross-linking agent. The coupling agent and the cross-linking agent make the epoxy resin adhesive in the ink and the polymer printing material produce a coupling body, thereby improving the fixing effect of the ink, reducing the film-forming temperature of the adhesive, and improving the adhesion of the ink. The ink is cured by the power of the UV light curing lamp. The curing wavelength of the UV lamp can be adjusted according to the different inks to achieve a better curing effect. During the production process of the yellow paper b, the drying temperature of the yellow paper b is 60-80°C, the drying time of the yellow paper b is 10-30 minutes, and the humidity of the dried yellow paper b is maintained at 15-25%. The thickness of the ink applied on the surface of the yellow paper b is 0.2mm-0.4mm. The yellow paper b is dyed and waxed. The yellow paper b is dyed by a coptis extract. The coptis extract increases the folding strength of the yellow paper b. The yellow paper b is coated with yellow wax. The yellow wax makes the paper smooth and firm. The black gold paper prepared by the preparation method of the novel black gold paper.

[0059] Embodiment 4: An embodiment provided by the present invention: A method for preparing a new type of black gold paper for gold foil forging, comprising the following steps:

[0060] Step s1, soaking and drying yellow paper a to form yellow paper b:

[0061] Step s2, applying ink on the surface of yellow paper b to form yellow paper c:

[0062] Step s3, coating the surface of yellow paper c with a temperature-resistant coating to form yellow paper d;

[0063] Step s4, placing the yellow paper d into a drying box for drying to form a substrate a:

[0064] Step s5, punching the substrate a to extend it to form a substrate b:

[0065] Step s6, cutting the substrate b to obtain black gold paper;

[0066] The heat-resistant coating comprises the following parts by weight of heat-resistant coating raw materials: 30 parts of silicon oxide, 30 parts of silicon carbide, 20 parts of silicone resin, 5 parts of stearic acid monoglyceride, 4 parts of oleic acid, 8 parts of myristyl alcohol, 7 parts of diethylenetriamine, and 120 parts of ultrapure water. The heat-resistant coating raw materials are formed by mixing and stirring. The heat-resistant coating raw materials are mixed through a reactor. The heat-resistant coating raw materials are filtered through a 30-mesh filter before mixing. The mixing time of the heat-resistant coating raw materials is 1.3 hours. The temperature of the heat-resistant coating raw materials when mixed is 35°C. The yellow paper a is made of young bamboo. The ink comprises bituminous coal and water. The bituminous coal is smoked on a smoke collection vessel generated by coal combustion. The quality of the bituminous coal is improved by adjusting the combustion temperature of the coal. After smoking, the bituminous coal is scraped off the collecting vessel. The bituminous coal is washed and filtered to remove impurities and excess water. The ink also comprises an epoxy resin adhesive. The epoxy resin adhesive has epoxy and reaction activity, and can form strong adhesion after cross-linking polymerization. The ink also includes a coupling agent and a cross-linking agent. The coupling agent and the cross-linking agent make the epoxy resin adhesive in the ink and the polymer printing material produce a coupling body, thereby improving the fixing effect of the ink, reducing the film-forming temperature of the adhesive, and improving the adhesion of the ink. The ink is cured by the power of the UV light curing lamp. The curing wavelength of the UV lamp can be adjusted according to the different inks to achieve a better curing effect. During the production process of the yellow paper b, the drying temperature of the yellow paper b is 60-80°C, the drying time of the yellow paper b is 10-30 minutes, and the humidity of the dried yellow paper b is maintained at 15-25%. The thickness of the ink applied on the surface of the yellow paper b is 0.2mm-0.4mm. The yellow paper b is dyed and waxed. The yellow paper b is dyed by a coptis extract. The coptis extract increases the folding strength of the yellow paper b. The yellow paper b is coated with yellow wax. The yellow wax makes the paper smooth and firm. The black gold paper prepared by the preparation method of the novel black gold paper.

[0067] Embodiment 5: An embodiment provided by the present invention: A method for preparing a new type of black gold paper for gold foil forging, comprising the following steps:

[0068] Step s1, soaking and drying yellow paper a to form yellow paper b:

[0069] Step s2, applying ink on the surface of yellow paper b to form yellow paper c:

[0070] Step s3, coating the surface of yellow paper c with a temperature-resistant coating to form yellow paper d;

[0071] Step s4, placing the yellow paper d into a drying box for drying to form a substrate a:

[0072] Step s5, punching the substrate a to extend it to form a substrate b:

[0073] Step s6, cutting the substrate b to obtain black gold paper;

[0074] The heat-resistant coating comprises the following parts by weight of heat-resistant coating raw materials: 35 parts of silicon oxide, 35 parts of silicon carbide, 24 parts of silicone resin, 6 parts of stearic acid monoglyceride, 5 parts of oleic acid, 9 parts of myristyl alcohol, 8 parts of diethylenetriamine, and 132 parts of ultrapure water. The heat-resistant coating raw materials are formed by mixing and stirring. The heat-resistant coating raw materials are mixed through a reactor. The heat-resistant coating raw materials are filtered through a 20-40 mesh filter before mixing. The mixing time of the heat-resistant coating raw materials is 1.8 hours. The temperature of the heat-resistant coating raw materials when mixed is 45°C. The yellow paper a is made of young bamboo. The ink comprises bituminous coal and water. The bituminous coal is smoked on a smoke collection vessel generated by coal combustion. The bituminous coal improves its quality by adjusting the combustion temperature of the coal. After smoking, the bituminous coal is scraped off the collection vessel. The bituminous coal is washed and filtered to remove impurities and excess water. The ink also comprises an epoxy resin adhesive. The epoxy resin adhesive has epoxy and reaction activity and can form strong adhesion after cross-linking polymerization. The ink also includes a coupling agent and a cross-linking agent. The coupling agent and the cross-linking agent make the epoxy resin adhesive in the ink and the polymer printing material produce a coupling body, thereby improving the fixing effect of the ink, reducing the film-forming temperature of the adhesive, and improving the adhesion of the ink. The ink is cured by the power of the UV light curing lamp. The curing wavelength of the UV lamp can be adjusted according to the different inks to achieve a better curing effect. During the production process of the yellow paper b, the drying temperature of the yellow paper b is 60 to 80°C, the drying time of the yellow paper b is 10 to 30 minutes, and the humidity of the dried yellow paper b is maintained at 15 to 25%. The thickness of the ink applied on the surface of the yellow paper b is 0.2 mm to 0.4 mm. The yellow paper b is dyed and waxed. The yellow paper b is dyed by a coptis extract. The coptis extract increases the folding strength of the yellow paper b. The yellow paper b is coated with yellow wax, and the yellow wax makes the paper smooth and firm. The black gold paper prepared by the preparation method of the novel black gold paper.

[0075] Comparative experiment:

[0076] The difference between Comparative Example 1 and Example 1 is that the heat-resistant coating comprises the following weight parts of heat-resistant coating raw materials: 22 parts of silicon oxide, 18 parts of silicon carbide, 15 parts of silicone resin, 5 parts of stearic acid monoglyceride, 2 parts of oleic acid, 4 parts of myristyl alcohol, 2 parts of diethylenetriamine, and 70 parts of ultrapure water, the heat-resistant coating raw materials are formed by mixing and stirring, the heat-resistant coating raw materials are mixed in a reactor, the heat-resistant coating raw materials are filtered through a 25-mesh filter before mixing, the heat-resistant coating raw materials are mixed for 1 hour, the temperature of the heat-resistant coating raw materials when mixed is 30°C, the yellow paper a is made of young bamboo, the ink comprises bituminous coal and water, the bituminous coal is smoked on a smoke collection vessel generated by coal combustion, and the bituminous coal The quality of bituminous coal is improved by adjusting the combustion temperature of coal. After smoking, the bituminous coal is scraped off the collecting container. The bituminous coal is washed and filtered to remove impurities and excess moisture. The ink also includes an epoxy resin adhesive. The epoxy resin adhesive has epoxy and reaction activity and can form strong adhesion after cross-linking polymerization. The ink also includes a coupling agent and a cross-linking agent. The coupling agent and the cross-linking agent make the epoxy resin adhesive in the ink and the polymer printing material produce a coupling body, thereby improving the fixing effect of the ink, and reducing the film-forming temperature of the adhesive, thereby improving the adhesion of the ink. The ink is cured by the power of a UV light curing lamp. The curing wavelength of the UV lamp can be adjusted according to the different inks to achieve a better curing effect.

[0077] The difference between Comparative Example 2 and Example 1 is that the heat-resistant coating comprises the following parts by weight of heat-resistant coating raw materials: 29 parts of silicon oxide, 32 parts of silicon carbide, 21 parts of silicone resin, 5 parts of stearic acid monoglyceride, 4 parts of oleic acid, 6 parts of myristyl alcohol, 6 parts of diethylenetriamine, and 90 parts of ultrapure water. The heat-resistant coating raw materials are formed by mixing and stirring. The heat-resistant coating raw materials are mixed in a reactor. Before mixing, the heat-resistant coating raw materials are filtered through a 20-40 mesh filter screen to filter impurities. The mixing time of the heat-resistant coating raw materials is 1.1 hours. The temperature of the heat-resistant coating raw materials when mixed is 40°C. The yellow paper a is made of young bamboo. The ink comprises bituminous coal and water. The bituminous coal is smoked on a smoke collection vessel generated by coal combustion. The bituminous coal is improved in quality by adjusting the combustion temperature of the coal. After smoking, the bituminous coal is scraped off the collecting container. The bituminous coal is washed and filtered to remove impurities and excess moisture. The ink also includes an epoxy resin adhesive. The epoxy resin adhesive has epoxy and reaction activity and can form strong adhesion after cross-linking polymerization. The ink also includes a coupling agent and a cross-linking agent. The coupling agent and the cross-linking agent make the epoxy resin adhesive in the ink and the polymer printing material produce a coupling body, thereby improving the fixing effect of the ink, and reducing the film-forming temperature of the adhesive, thereby improving the adhesion of the ink. The ink is cured by the power of the UV light curing lamp. The curing wavelength of the UV lamp can be adjusted according to the different inks to achieve better curing effects.

[0078] The difference between Comparative Example 3 and Example 1 is that the heat-resistant coating comprises the following parts by weight of heat-resistant coating raw materials: 28 parts of silicon oxide, 32 parts of silicon carbide, 20 parts of silicone resin, 4 parts of stearic acid monoglyceride, 3 parts of oleic acid, 7 parts of myristyl alcohol, 7 parts of diethylenetriamine, and 120 parts of ultrapure water, the heat-resistant coating raw materials are formed by mixing and stirring, the heat-resistant coating raw materials are mixed in a reactor, the heat-resistant coating raw materials are filtered through a 28-mesh filter before mixing, the heat-resistant coating raw materials are mixed for 1.6 hours, the temperature of the heat-resistant coating raw materials when mixed is 28°C, the yellow paper a is made of young bamboo, the ink comprises bituminous coal and water, and the bituminous coal is smoked on a smoke collection vessel generated by coal combustion, The bituminous coal improves its quality by adjusting the combustion temperature of the coal. After smoking, the bituminous coal is scraped off the collecting container. The bituminous coal is washed and filtered to remove impurities and excess moisture. The ink also includes an epoxy resin adhesive. The epoxy resin adhesive has epoxy and reaction activity and can form strong adhesion after cross-linking polymerization. The ink also includes a coupling agent and a cross-linking agent. The coupling agent and the cross-linking agent make the epoxy resin adhesive in the ink and the polymer printing material produce a coupling body, thereby improving the fixing effect of the ink, and reducing the film-forming temperature of the adhesive, thereby improving the adhesion of the ink. The ink is cured by the power of a UV light curing lamp. The curing wavelength of the UV lamp can be adjusted according to the different inks to achieve a better curing effect.

[0079] The difference between Comparative Example 4 and Example 1 is that the heat-resistant coating comprises the following parts by weight of heat-resistant coating raw materials: 30 parts of silicon oxide, 30 parts of silicon carbide, 20 parts of silicone resin, 5 parts of stearic acid monoglyceride, 4 parts of oleic acid, 8 parts of myristyl alcohol, 7 parts of diethylenetriamine, and 120 parts of ultrapure water, the heat-resistant coating raw materials are formed by mixing and stirring, the heat-resistant coating raw materials are mixed by a reactor, the heat-resistant coating raw materials are filtered through a 30-mesh filter before mixing, the heat-resistant coating raw materials are mixed for 1.3 hours, the temperature of the heat-resistant coating raw materials when mixed is 35°C, the yellow paper a is made of young bamboo, the ink comprises bituminous coal and water, and the bituminous coal is smoked on a smoke collection vessel generated by coal combustion, The bituminous coal improves its quality by adjusting the combustion temperature of the coal. After smoking, the bituminous coal is scraped off the collecting container. The bituminous coal is washed and filtered to remove impurities and excess moisture. The ink also includes an epoxy resin adhesive. The epoxy resin adhesive has epoxy and reaction activity and can form strong adhesion after cross-linking polymerization. The ink also includes a coupling agent and a cross-linking agent. The coupling agent and the cross-linking agent make the epoxy resin adhesive in the ink and the polymer printing material produce a coupling body, thereby improving the fixing effect of the ink, and reducing the film-forming temperature of the adhesive, thereby improving the adhesion of the ink. The ink is cured by the power of a UV light curing lamp. The curing wavelength of the UV lamp can be adjusted according to the different inks to achieve a better curing effect.

[0080] The difference between Comparative Example 5 and Example 1 is that the heat-resistant coating comprises the following parts by weight of heat-resistant coating raw materials: 35 parts of silicon oxide, 35 parts of silicon carbide, 24 parts of silicone resin, 6 parts of stearic acid monoglyceride, 5 parts of oleic acid, 9 parts of myristyl alcohol, 8 parts of diethylenetriamine, and 132 parts of ultrapure water. The heat-resistant coating raw materials are formed by mixing and stirring. The heat-resistant coating raw materials are mixed in a reactor. Before mixing, the heat-resistant coating raw materials are filtered through a 20-40 mesh filter screen to filter impurities. The mixing time of the heat-resistant coating raw materials is 1.8 hours. The temperature of the heat-resistant coating raw materials when mixed is 45°C. The yellow paper a is made of young bamboo. The ink comprises bituminous coal and water. The bituminous coal is smoked on a smoke collection vessel generated by coal combustion. The bituminous coal is improved in quality by adjusting the combustion temperature of the coal. After smoking, the bituminous coal is scraped off the collecting container. The bituminous coal is washed and filtered to remove impurities and excess moisture. The ink also includes an epoxy resin adhesive. The epoxy resin adhesive has epoxy and reaction activity and can form strong adhesion after cross-linking polymerization. The ink also includes a coupling agent and a cross-linking agent. The coupling agent and the cross-linking agent make the epoxy resin adhesive in the ink and the polymer printing material produce a coupling body, thereby improving the fixing effect of the ink, and reducing the film-forming temperature of the adhesive, thereby improving the adhesion of the ink. The ink is cured by the power of the UV light curing lamp. The curing wavelength of the UV lamp can be adjusted according to the different inks to achieve better curing effects.

[0081] The black gold paper of Example 1, Example 2, Example 3, Example 4, and Example 5 of the present invention and the traditional black gold paper (Comparative Example 1) were respectively taken out to conduct tensile strength test, gold foil yield rate, black gold paper utilization rate and gold foil consumption grams, and their values ​​were calculated and statistically analyzed. The results are shown in Table 1:

[0082] Tensile strength (N / mm2) Gold foil yield rate (%) Utilization rate of black gold paper (%) Gold consumption per 10,000 sheets of gold foil (g) Example 1 5 95 98 189 Example 2 6 96 98 190 Example 3 4 97 99 191 Example 4 5 96 98 188 Example 5 5 98 98 192 Comparative Example 1 2 60 50 220

[0083] Table 1

[0084] From the data in Table 1, it can be seen that the tensile strength coefficients of the black gold paper in Example 1, Example 2, Example 3, Example 4 and Example 5 of the present invention are 5, 6, 4, 5 and 5 respectively, which are significantly higher than the tensile strength coefficient of the black gold paper in Comparative Example 1. Therefore, it is shown that compared with traditional paper, the tensile strength of the black gold paper of the present invention is significantly improved, the service life is increased by 1-3 times, and the foil extension speed is more than doubled.

[0085] From the data in Table 1, it can be seen that the gold foil yield rates of the black gold paper using Examples 1, 2, 3, 4 and 5 of the present invention are 95, 96, 97, 96 and 98 respectively, which are significantly higher than the gold foil yield rate of the black gold paper in Comparative Example 1. This indicates that the gold foil yield rate of the black gold paper of the present invention is significantly improved compared with traditional paper.

[0086] From the data in Table 1, it can be seen that the utilization rates of the black gold paper using the black gold paper in Example 1, Example 2, Example 3, Example 4 and Example 5 of the present invention are 98, 98, 99, 98 and 98 respectively, which are significantly higher than the utilization rate of the black gold paper in Comparative Example 1. Therefore, it is shown that the utilization rate of the black gold paper of the present invention is significantly improved compared with traditional paper.

[0087] From the data in Table 1, it can be seen that the grams of gold foil consumed by the black gold paper in Examples 1, 2, 3, 4 and 5 of the present invention are 198, 190, 191, 188 and 192 respectively, which are significantly lower than the grams of gold foil consumed by the black gold paper in Comparative Example 1. Therefore, it is shown that the grams of gold foil consumed by the black gold paper of the present invention is significantly reduced compared with traditional paper.

[0088] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing a new type of black gold paper for gold foil forging, characterized in that: The following steps are involved: Step s1, soaking and drying yellow paper a to form yellow paper b: Step s2, applying ink on the surface of yellow paper b to form yellow paper c: Step s3, coating the surface of yellow paper c with a temperature-resistant coating to form yellow paper d; Step s4, placing the yellow paper d into a drying box for drying to form a substrate a: Step s5, punching the substrate a to extend it to form a substrate b: Step s6, cutting the substrate b to obtain black gold paper; The heat-resistant coating comprises the following raw materials of the heat-resistant coating in parts by weight: 20 to 35 parts of silicon oxide, 15 to 35 parts of silicon carbide, 13 to 24 parts of silicone resin, 4 to 6 parts of stearic acid monoglyceride, 2 to 5 parts of oleic acid, 3 to 9 parts of myristyl alcohol, 2 to 8 parts of diethylenetriamine and 65 to 132 parts of ultrapure water. The raw materials of the heat-resistant coating are formed by mixing and stirring. The raw materials of the heat-resistant coating are mixed in a reactor. Before mixing, the raw materials of the heat-resistant coating are filtered for impurities through a 20 to 40 mesh filter screen. The mixing time of the raw materials of the heat-resistant coating is 1 to 1.8 hours, and the temperature of the raw materials of the heat-resistant coating when mixed is 25 to 45°C.

2. The method for preparing a new type of black gold paper for gold foil forging according to claim 1, characterized in that: The yellow paper a is made of young bamboo.

3. The method for preparing a new type of black gold paper for gold foil forging according to claim 1, characterized in that: The ink includes bituminous coal and water. The bituminous coal is smoked on a smoke collecting container generated by coal combustion. The bituminous coal quality is improved by adjusting the combustion temperature of the coal. After smoking, the bituminous coal is scraped off the collecting container. The bituminous coal is washed and filtered to remove impurities and excess water.

4. The method for preparing a new type of black gold paper for gold foil forging according to claim 3, characterized in that: The ink also includes an epoxy resin adhesive, which has epoxy and reaction activity and can form strong adhesion after cross-linking polymerization.

5. The method for preparing a new type of black gold paper for gold foil forging according to claim 4, characterized in that: The ink also includes a coupling agent and a cross-linking agent, which couple the epoxy resin adhesive in the ink with the polymer printing material to form a coupling body, thereby improving the fixing effect of the ink, reducing the film-forming temperature of the adhesive, and improving the adhesion of the ink. The ink is cured by the power of a UV curing lamp, and the curing wavelength of the UV lamp can be adjusted according to the different inks to achieve a better curing effect.

6. The method for preparing a new type of black gold paper for gold foil forging according to claim 1, characterized in that: During the production process of the yellow paper b, the drying temperature of the yellow paper b is 60-80° C., the drying time of the yellow paper b is 10-30 minutes, and the humidity of the dried yellow paper b is maintained at 15-25%.

7. The method for preparing a new type of black gold paper for gold foil forging according to claim 1, characterized in that: The ink is applied to the surface of yellow paper b to a thickness of 0.2 mm to 0.4 mm.

8. The method for preparing a new type of black gold paper for gold foil forging according to claim 1, characterized in that: The yellow paper b is dyed and waxed, and the yellow paper b is dyed by the Phellodendron chinense extract, and the Phellodendron chinense extract increases the folding strength of the yellow paper b.

9. The method for preparing a new type of black gold paper for gold foil forging according to claim 8, characterized in that: The yellow paper b is coated with yellow wax, which makes the paper smooth and firm.

10. A novel black gold paper for gold foil forging, suitable for the preparation method of the novel black gold paper for gold foil forging according to any one of claims 1 to 9, characterized in that: The black gold paper is made by the preparation method of the novel black gold paper.

Citation Information

Patent Citations

  • Method for preparing coal paper and special black smock adhesive

    CN101446056A

  • Black oil coated paper for making metal foil

    CN2263129Y