Response surface theory-based geopolymer-based composite repair mortar multi-parameter performance prediction method

By optimizing the mix proportion of geopolymer composite repair mortar using response surface methodology, the problems of high energy consumption and insufficient corrosion resistance of cement-based repair materials were solved. This resulted in the preparation of a repair mortar with excellent mechanical and durability properties, suitable for trenchless repair of underground pipe networks, achieving low-carbon and environmentally friendly construction results.

CN119049598APending Publication Date: 2024-11-29SHANGHAI URBAN CONSTRUCTION DESIGN & RESEARCH INSTITUTE (GROUP) CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410496235.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-24
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The cement-based repair materials used in traditional trenchless repair technologies suffer from high energy consumption, high carbon emissions, and insufficient corrosion resistance, which limits their application scenarios. Furthermore, traditional geopolymer-based repair mortars have drawbacks in terms of large shrinkage and material brittleness.

Method used

Using the central composite design method of response surface theory and the DesignExpert software platform, experimental design and visualization analysis were conducted to optimize the mix proportion of the geopolymer composite repair mortar. The mortar was modified with polypropylene fiber, cement-based penetrating crystallizing material and hydroxypropyl methylcellulose to prepare a repair mortar with excellent mechanical properties and durability.

Benefits of technology

It significantly reduced the workload of experiments, improved the accuracy and reliability of performance prediction, and the prepared geopolymer-based composite repair mortar achieved a compressive strength of over 70 MPa at room temperature after 28 days, a fluidity of over 200 mm, and a shrinkage value of less than 1‰ after 7 days, thus expanding the application scenarios and reducing the environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119049598A_ABST
    Figure CN119049598A_ABST
Patent Text Reader

Abstract

The invention discloses a geopolymer-based composite repair mortar multi-parameter performance prediction method based on a response surface theory. The geopolymer-based composite repair mortar multi-parameter performance prediction method comprises the following steps: (1) determining a basic formula of geopolymer-based composite repair mortar; (2) determining a set range of variables by utilizing a single-factor test, and designing a mix proportion; (3) stirring and pouring the geopolymer-based composite repair mortar, and obtaining a response value by adopting a test mode; (4) performing quadratic model fitting on the main variable and the response value to obtain a quadratic polynomial regression equation; (5) performing analysis and significance verification on a fitting result; (6) setting an expected value, and solving the optimal mix proportion by using a response surface equation; and (7) testing by utilizing the mode in the step (3), and verifying the accuracy of the optimal solution in the step (6). The method provided by the invention has the advantages of less workload, more intuitive analysis chart and lower prediction error. The optimized repair mortar provided by the invention has better mechanical and durability properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of novel green building materials and pipeline trenchless repair engineering repair mortar, and in particular to a multi-parameter performance prediction method for geopolymer-based composite repair mortar based on response surface theory. Background Art

[0002] Traditional underground pipe network repair work generally adopts the repair method of excavation-pipe replacement, which will cause damage to the original roads during construction and greatly affect the city's traffic and environment. Construction in complex cities not only requires large capital investment and is difficult, but also involves multiple related units, resulting in huge compensation costs. Trenchless repair technology uses the inspection well of the original pipeline as the construction entrance, and conducts targeted repairs on defective parts according to the actual situation of the underground pipe network. This technology can not only avoid the impact of excavation-pipe replacement on traffic and environment in large cities, but also has greater advantages in cost and construction safety compared to traditional excavation repair.

[0003] Generally, the repair mortar used in traditional trenchless repair technology is a cement-based repair material. Due to the mature cement industry chain, although it has a great advantage in cost, its high energy consumption, high carbon emissions and high pollution production methods are not conducive to the country's "dual carbon" strategy. In addition, the cement-based itself is not resistant to acid and alkali corrosion, which limits its application scenarios. Compared with cement-based repair materials, geopolymer-based composite repair mortar has excellent mechanical properties and corrosion resistance, abundant raw materials, and can utilize solid waste resources, truly achieving low carbon and environmental protection.

[0004] Technicians in this technical field are committed to solving the above-mentioned technical defects. Summary of the invention

[0005] In view of the above-mentioned defects of the prior art, the technical purpose of the present invention is that the technical solution adopted by the present invention is to realize experimental design by using the central composite design method (Box-Behnken, BBD for short) based on the response surface theory, and to conduct experiments based on the DesignExpert software platform using preset variables to obtain response values ​​for visual analysis, and to set global expected values, so as to finally obtain the optimal predicted value of the mix ratio of geopolymer composite repair mortar.

[0006] To achieve the above technical objectives, the present invention provides the following technical solutions: A multi-parameter performance prediction method of geopolymer-based composite repair mortar based on response surface theory of the present invention comprises the following steps:

[0007] (1) Determine the basic formula of geopolymer-based composite repair mortar, including the configuration of aggregate, geopolymer precursor and alkaline activator;

[0008] (2) Use single factor experiments to determine the setting range of each variable and design several groups of geopolymer-based composite repair mortar mix ratios;

[0009] (3) mixing and pouring the geopolymer-based composite repair mortar, and obtaining the response value by means of an experimental method;

[0010] (4) Fitting a quadratic model to the main variable and the response value to obtain a quadratic polynomial regression equation;

[0011] (5) Analyze the fitting results and verify their significance;

[0012] (6) Set the expected value and use the response surface equation to solve the optimal mix ratio;

[0013] (7) Conduct an experiment using the method of step (3) to verify the accuracy of the optimal solution of step (6).

[0014] Furthermore, in step (1), the type and particle size of the aggregate, the type and fineness of the geopolymer precursor, and the type, modulus and concentration of the alkaline activator are used as preset parameters.

[0015] Furthermore, in step (2), the variables include the types and dosages of polypropylene fiber PPF, cement-based infiltrative crystallization material CCCW, and hydroxypropyl methylcellulose HPMC.

[0016] Furthermore, in step (3), the molding method of the geopolymer composite repair mortar includes first dry-mixing the geopolymer precursor and the main variable for a preset time, then adding an alkaline activator and stirring for a preset time to obtain a slurry, pouring the mixture slurry into a mold, waiting for a preset time to demold, and standard curing until a preset time. The test method adopts a compression test, a flexural test, and an expansion and contraction test.

[0017] Furthermore, in step (4), the measured data were fitted with a quadratic model of the response surface method using multiple nonlinear fitting, and the dosages of HPMC (A), CCCW (B) and PPF (C) were used as variables to obtain quadratic polynomial regression equations for compressive strength Y1, fluidity Y2 and 7d shrinkage value Y3, as shown in equations (1) to (3):

[0018] Y1=75.05-0.9675*A-1.16*B+0.6437*C-0.5025*AB+0.2075*AC-0.32*BC+0.1835*A2-1.88*B2-1.95*C2(1)

[0019] Y2=194.64-2.9*A+1.2*B-14.8*C-1.25*AB+4.85*AC+1.5*BC-1.95*A2+3.55*B2+4.31*C2(2)

[0020] Y3=127-16.63*A-2.75*B-10.88*C-24.75*AB+9.5*AC+2.75*BC+47.25A2+22B2-21.25*C2(3).

[0021] Furthermore, in step (6), the expected values ​​and the optimized dosages of polypropylene fiber PPF, cement-based permeable crystallization material CCCW, and hydroxypropyl methylcellulose HPMC are set; in step (7), the verification method, verification value, and error adopted for the optimal mix ratio are set.

[0022] Furthermore, in step (1), the geopolymer-based composite repair mortar comprises the following components in parts by weight:

[0023]

[0024] The alkaline activator is a mixture of sodium silicate Na2SiO3 and sodium hydroxide NaOH, wherein the modulus of sodium silicate is 2.3, the concentration is 43.5%, the mass fraction ratio of SiO2 is 29.99%, the mass fraction ratio of Na2O is 13.75%, and the purity of sodium hydroxide is 99%. By mass, 104 parts of sodium hydroxide are dissolved in 250 parts of water to prepare a sodium hydroxide solution. After the solution is cooled, it is mixed with 650 parts of sodium silicate, stirred thoroughly, and left to stand for 12 hours for use.

[0025] The cement-based penetrating crystal material used is Xypex admixture from Beijing Chengrong Waterproof Material Co., Ltd., and hydroxypropyl methylcellulose is purchased from Hebei Weiteng Building Materials Co., Ltd., with a molecular weight (degree of polymerization) of 200,000. The cement-based penetrating material is purchased on the market, from Xypex admixture from Beijing Chengrong Waterproof Material Co., Ltd., and hydroxypropyl methylcellulose is purchased on the market, from Hebei Weiteng Building Materials Co., Ltd.

[0026] Furthermore, in step (1), the method for preparing the geopolymer-based composite repair mortar comprises the following steps:

[0027] Step 1: Use 800-mesh metakaolin as the geopolymer precursor. Add 650 parts of metakaolin by weight to the preset mass percentage of polypropylene PP fiber, cement-based infiltration crystallization material and hydroxypropyl methylcellulose to the precursor and pre-mix for 3 minutes.

[0028] Step 2: Add 500 parts of the prepared and aged alkaline activator to the geopolymer precursor and stir at low speed for 2 minutes, then add 1350 parts of Chinese IOS standard sand and stir at high speed for 3 minutes to obtain a slurry;

[0029] Step 3: Load the slurry obtained in step 2 into an expansion and contraction instrument for testing or into a 160mm*40mm*40mm plastic test mold, and vibrate it for 2 minutes using a cement mortar vibrator with a vibration frequency of 1Hz. Scrape it until it is still and wait for 24 hours before demoulding. Transfer it to a standard curing room for curing for a predetermined time to obtain a geopolymer-based composite repair mortar specimen.

[0030] Furthermore, in step (7), the test blocks after the predetermined curing time are subjected to compressive and flexural strength tests to obtain response values, which are input into the Design Expert software platform together with the response values ​​of expansion and contraction for response surface analysis. The interaction and significance level of each variable in the response value are analyzed using significance test, and P value < 0.05 is significant. The global expectation of 28d compressive strength and fluidity is set to be large, and the shrinkage value is expected to be small, and the optimal mix ratio with comprehensive performance is solved and verified by the above experiment. The error is compared. If the error is < 5%, it is considered that the predicted value is consistent with the actual value. Otherwise, the above steps are repeated.

[0031] The geopolymer-based composite repair mortar prepared by the method of the invention.

[0032] Beneficial effects: The cement-based repair mortar of the present invention has more excellent mechanical properties and durability. The advantage of the present invention is that it reduces the workload of the experiment. Through the application of response surface theory, intuitive analysis charts are provided, making the performance prediction more intuitive and easy to understand. At the same time, the method can significantly reduce the prediction error and improve the accuracy of the prediction. The cement-based repair mortar optimized by this method will have more excellent mechanical properties and durability, thereby showing higher reliability and long life in practical applications.

[0033] Compared with the prior art, the present invention has the following advantages:

[0034] (1) An experimental design method based on response surface theory was used to predict the optimal mix ratio under multivariable conditions. Compared with traditional single-factor and orthogonal experiments, it has less workload, more intuitive analysis charts and lower prediction errors.

[0035] (2) The present invention aims to improve the shortcomings of traditional geopolymer-based repair mortars, such as large shrinkage and brittle materials, by using PP fibers, cement-based permeable crystallization materials, and hydroxypropyl methylcellulose to modify the mortar, making it more suitable for various application scenarios in trenchless repair construction of underground pipe networks. The geopolymer-based composite repair mortar prepared by the present invention has excellent mechanical properties and working performance. The 28d compressive strength at room temperature can reach more than 70Mpa, the fluidity can reach more than 200mm, and the 7d shrinkage value can be less than 1‰.

[0036] (3) The geopolymer-based composite repair mortar prepared by the present invention has better mechanical properties and durability than the traditional cement-based repair mortar. In terms of corrosion resistance, the present invention solves the shortcomings of poor durability of traditional cement-based mortars in corrosive sewage pipes and expands the application scenarios of repair mortars. Compared with cement materials, geopolymer-based repair mortars have the advantages of low energy consumption, low carbon emissions and low environmental pollution. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a diagram showing the influence of various variables on the mechanical properties of geopolymer-based repair mortar in the single factor experiment of the present invention.

[0038] Figure 2 This is a scanning electron microscope (SEM) image of the PP fiber incorporated into the present invention.

[0039] Figure 3 This is the XRD diagram of the sample doped with CCCW and HPMC in the present invention.

[0040] Figure 4 This is the TF-IR graph of the sample doped with CCCW and HPMC according to the present invention.

[0041] Figure 5 This is the mercury injection increment diagram of the HPMC samples with different dosages of the present invention.

[0042] Figure 6 This is a comparison chart of the TG-DTG spectra of the sample doped with CCCW and the blank sample of the present invention. DETAILED DESCRIPTION

[0043] The concept, specific structure and technical effects of the present invention will be further described below in conjunction with the accompanying drawings to fully understand the purpose, characteristics and effects of the present invention.

[0044] The present invention will be further described in detail below through the accompanying drawings and specific embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0045] Example 1

[0046] A multi-parameter performance prediction method for geopolymer-based composite repair mortar based on response surface theory of the present invention comprises the following steps:

[0047] (1) Determine the basic formula of geopolymer-based composite repair mortar, including the configuration of aggregate, geopolymer precursor and alkaline activator; the type and particle size of aggregate, the type and fineness of geopolymer precursor, the type, modulus and concentration of alkaline activator are used as preset parameters.

[0048] The geopolymer-based composite repair mortar comprises the following components in parts by weight:

[0049]

[0050] The alkaline activator is a mixture of sodium silicate Na2SiO3 and sodium hydroxide NaOH, wherein the modulus of sodium silicate is 2.3, the concentration is 43.5%, the mass fraction ratio of SiO2 is 29.99%, the mass fraction ratio of Na2O is 13.75%, and the purity of sodium hydroxide is 99%. According to the mass fraction, 104 parts of sodium hydroxide are dissolved in 250 parts of water to prepare a sodium hydroxide solution, and after the solution is cooled, it is mixed with 650 parts of sodium silicate, fully stirred and left to stand for 12 hours for use.

[0051] The preparation method of geopolymer-based composite repair mortar comprises the following steps:

[0052] Step 1: Use 800-mesh kaolin as the precursor. Add 650 parts of kaolin by weight to the preset mass percentage of polypropylene PP fiber, cement-based infiltration crystallization material and hydroxypropyl methylcellulose to the precursor and pre-mix for 3 minutes.

[0053] Step 2: Add 500 parts of the prepared and aged alkaline activator to the geopolymer precursor and stir at low speed for 2 minutes, then add 1350 parts of Chinese IOS standard sand and stir at high speed for 3 minutes to obtain a slurry;

[0054] Step 3: Load the slurry into an expansion and contraction instrument for testing or into a 160mm*40mm*40mm plastic test mold, and vibrate it for 2 minutes using a cement mortar vibrator with a vibration frequency of 1Hz. Scrape it until it is still and wait for 24 hours before demolding. Transfer it to a standard curing room for curing for a predetermined time to obtain a geopolymer-based composite repair mortar.

[0055] (2) Single-factor experiments were used to determine the setting range of each variable and design the mix ratios of several groups of geopolymer-based composite repair mortars; the variables included the type and dosage of polypropylene fiber (PPF), cement-based penetrating crystallization material (CCCW), and hydroxypropyl methylcellulose (HPMC).

[0056] (3) The geopolymer-based composite repair mortar is stirred and poured, and the response value is obtained by a test method; the molding method of the geopolymer composite repair mortar includes first dry-mixing the geopolymer precursor and the main variable for a preset time, then adding an alkaline activator and stirring for a preset time to obtain a slurry, pouring the mixture slurry into a mold, waiting for a preset time to remove the mold, and standard curing until a preset time. The test method adopts a compression test, a flexural test, and an expansion and contraction test.

[0057] (4) A quadratic model is fitted for the main variable and the response value to obtain a quadratic polynomial regression equation; the quadratic model of the response surface method is used to perform multivariate nonlinear fitting on the measured data to obtain the quadratic polynomial regression equations of compressive strength Y1, fluidity Y2 and 7d shrinkage value Y3, as shown in equations (1) to (3):

[0058] Y1=75.05-0.9675*A-1.16*B+0.6437*C-0.5025*AB+0.2075*AC-0.32*BC+0.1835*A2-1.88*B2-1.95*C2(1)

[0059] Y2=194.64-2.9*A+1.2*B-14.8*C-1.25*AB+4.85*AC+1.5*BC-1.95*A2+3.55*B2+4.31*C2(2)

[0060] Y3=127-16.63*A-2.75*B-10.88*C-24.75*AB+9.5*AC+2.75*BC+47.25A2+22B2-21.25*C2(3).

[0061] (5) Analyze the fitting results and verify their significance;

[0062] (6) setting expected values ​​and solving the optimal mix ratio using the response surface equation; the set expected values ​​and the optimized dosages of polypropylene fiber PPF, cement-based permeable crystallization material CCCW, and hydroxypropyl methylcellulose HPMC;

[0063] (7) Conduct an experiment using the method of step (3) to verify the accuracy of the optimal solution of step (6). Verification method, verification value and error adopted for the optimal mix ratio. After reaching the predetermined curing time, the test blocks are subjected to compressive and flexural strength tests to obtain response values, which are input into the Design Expert software platform together with the response values ​​of expansion and shrinkage for response surface analysis. The interaction and significance level of each variable in the response value are analyzed using significance test, and P value <0.05 is significant; set the global expectation of 28d compressive strength, fluidity and shrinkage value to be large, solve for the mix ratio with the best comprehensive performance, and use the above experiment for verification, compare the errors, and if the error is <5%, it is considered that the predicted value is consistent with the actual value, otherwise repeat the above steps.

[0064] Test Example 1

[0065] 1. Single Factor Experiment

[0066] In the early stage of experimental design, single factor experiments were used to explore the effects of HPMC, CCCW and PPF on the 3d and 7d compressive strength of geopolymer mortar at different dosages. HPMC dosage, CCCW dosage and PFF dosage were selected as independent variable factors, represented by A1, A2 and A3 respectively, and the 28d compressive strength, fluidity and 7d shrinkage value of the mortar were response values, represented by Y1, Y2 and Y3 respectively. Figure 1 As shown, after comprehensive consideration, the level of independent variable factor A1 was determined to be 0.2%~0.6%, the level of A2 was 0.6%~1%, and the level of A3 was 0.4%~0.8%. A three-factor three-level experiment was conducted, and the upper, middle, and lower levels of each factor were coded with 1, 0, and -1, where -1 is a low level, 0 is the center point, and +1 is a high level. The specific values, coding and levels of the experimental independent variable factors are shown in Table 1.

[0067] Table 1

[0068]

[0069] Test Example 2

[0070] 2. Test methods

[0071] Compressive strength test: According to GB / T 17671-2021 "Test method for strength of cement mortar (ISO method)", the TYE-600E fully automatic compressive strength tester is used to test the compressive strength of the formed specimens.

[0072] Fluidity test: According to GB / T 2419-2005 “Determination method of fluidity of cement mortar”, the fluidity of mortar was tested using NLD-3 mortar fluidity tester.

[0073] Shrinkage test: The mortar drying shrinkage test was carried out using the Leichter / Guanya mortar expansion and contraction instrument. The test block specifications were 40mm×40mm×160mm, the acquisition rate was 5s / time, and the acquisition accuracy was 0.001mm.

[0074] Microscopic test: SEM test was performed using Apreo 2 scanning electron microscope from Thermo Fisher. XRD test was performed using smartlab9 X-ray diffractometer from Rigaku Corporation, Japan, with a diffraction angle 2θ scanning range of 10°-90°. Infrared spectrum test was performed using Nicolet-iS10 Fourier transform infrared spectrometer from Thermo Fisher. Thermogravimetric analysis was performed using NETZSCH STA 449F3 from NETZSCH, Germany. Mercury intrusion test was performed using MicroActive AutoPore V 9620 mercury intrusion instrument from Mack, USA.

[0075] 3. Experimental plan and results

[0076] According to the Box-Behnken experimental design, there are 17 groups of experimental points, each group has 3 experiments for flexural strength and 6 experiments for compression. The average value of the experimental data is taken as the experimental result. After the experiment, the measured data of the specimen's compression, flexural strength and fluidity are shown in Table 2.

[0077] Table 2

[0078]

[0079] 4. Regression equation

[0080] The quadratic model of the response surface methodology was used to perform multivariate nonlinear fitting on the measured data in Table 3. The dosages of HPMC (A), CCCW (B) and PPF (C) were used as variables to obtain quadratic polynomial regression equations for compressive strength Y1, fluidity Y2 and 7d shrinkage value Y3, as shown in Equations (1) to (3).

[0081] Y1=75.05-0.9675*A-1.16*B+0.6437*C-0.5025*AB+0.2075*AC-0.32*BC+0.1835*A2-1.88*B2-1.95*C2(1)

[0082] Y2=194.64-2.9*A+1.2*B-14.8*C-1.25*AB+4.85*AC+1.5*BC-1.95*A2+3.55*B2+4.31*C2(2)

[0083] Y3=127-16.63*A-2.75*B-10.88*C-24.75*AB+9.5*AC+2.75*BC+47.25A2+22B2-21.25*C2(3)

[0084] 5. ANOVA

[0085] The Design Expert software was used to perform regression model variance analysis on the 28d compression strength, 28d flexural strength and 7d shrinkage values. The results of the response surface regression model variance analysis table are shown in Table 3.

[0086] Table 3

[0087]

[0088] In the response surface model, the significance test of the parameters will be performed. It is generally believed that a P-value greater than 0.05 is not significant, a P-value greater than 0.0001 and less than 0.05 is significant, and a P-value less than 0.0001 is very significant. The smaller the P-value of the overall model, the more significant the relationship between the parameter and the response value. The lack of fit test is used to determine whether the random error of the data in the model is reasonably fitted. The larger the P-value of the lack of fit test, the less significant it is, and the smaller the probability of error in the model.

[0089] It can be seen from Table 3 that in the overall model of 28d compressive strength, fluidity and shrinkage value, the P value is less than 0.0001, indicating that this model is very significant and the fitting accuracy is very high, while the P value of the lack-of-fit test is greater than 0.05, indicating that the lack-of-fit is not significant and the probability of error in the model is small.

[0090] As shown in Table 5, the P values ​​of HPMC, CCCW and PPF in the compressive strength model are all less than 0.05. It can be considered that the three factors have a great influence on the compressive strength, and the influence of the three factors on the compressive strength is ranked as CCCW>HPMC>PPF.

[0091] In the overall model of fluidity, the P values ​​of the three factors HPMC, CCCW, and PPF are all less than 0.0001, which is very significant; this proves that HPMC, CCCW, and PPF have a relatively large impact on fluidity, and the F value of PPF is 29426.83, which is much larger than the other two factors. Therefore, the impact on fluidity is ranked as PPF>HPMC>CCCW.

[0092] In the overall model of 7d shrinkage value, the P values ​​of HPMC and PPF are both less than 0.0001, which proves that HPMC and PPF have a greater impact on the 7d shrinkage of mortar, while the P value of CCCW is 0.0483, which is close to the insignificant 0.05. It can be considered that CCCW has little effect on the 7d shrinkage of mortar. The influence of the three factors on the 7d shrinkage of mortar is ranked as HPMC>PPF>CCCW.

[0093] 6. Optimal mix ratio

[0094] To further verify the validity of the regression model and the accuracy of the prediction results, the credibility and quality of the model are evaluated through the Fit Statistics table in the software. It can be seen from Table 4 that in the 28d compressive strength, fluidity, and 7d shrinkage value models, the variance of the experimental data is very close to 1 and the coefficient of variation (CV%) is less than 10, which proves that the experimental fit is very good and the error is low. The Fit Statistics table is shown in Table 4:

[0095] Table 4

[0096]

[0097] The response surface model can be optimized using Design-Expert software. After optimization, it is concluded that the three factors of HPMC, CCCW and PPF have an optimal ratio in terms of the compressive strength, fluidity and drying shrinkage of geopolymer repair mortar, so as to achieve the best effect of multi-factor synergy. It can be seen from Table 5 that the prediction is optimal when the HPMC dosage is 0.306%, the CCCW dosage is 0.764% and the PPF dosage is 0.423%, and the predicted values ​​of 28d compressive strength, fluidity and 7d shrinkage are 73.6Mpa, 213.45mm and 133.98um. After experimental verification, the measured 28d compressive strength, fluidity and 7d shrinkage values ​​are 71.9Mpa, 211.25mm and 128um respectively. The errors are 2.3%, 1.03% and 4.5% respectively, which proves that the optimization and prediction accuracy of the mix ratio using the response surface method is high.

[0098] The comparison table between prediction and actual measurement is shown in Table 5:

[0099] Table 5

[0100]

[0101] Test Example 3

[0102] 3 Microscopic mechanism of action

[0103] 3.1 Scanning electron microscopy (SEM) analysis

[0104] like Figure 2 As shown, Figure 2 This is a scanning electron microscope (SEM) image of the PP fiber incorporated in the present invention. Through the scanning electron microscope (SEM), it can be found that Figure 2 In (a), the N(C)-ASH gel tightly wraps the fibers together to form a skeleton-filling structure, which makes the slurry more tightly bonded, increases its integrity, and reduces the probability of defects. Figure 2 As can be seen in (b), cracks are generated when the mortar is stressed or dried. The addition of PPF can effectively share part of the stress and restrict the generation and development of cracks. This is consistent with the previous analysis that PPF can increase the compressive strength of the mortar and reduce the drying shrinkage value. However, since the surface of the fiber is relatively smooth, the bonding friction generated is not enough to resist the huge stress that causes cracks, which will cause the slurry and fiber to peel off, and the strengthening effect on the mortar is limited, and the expected effect cannot be achieved.

[0105] The addition of an appropriate amount of PP fiber can enhance the compressive strength and shrinkage of the mortar, while excessive fiber will also have some adverse effects. Figure 2 (c) The agglomeration of fibers inside the mortar can be clearly seen. The entanglement of the long and thin fibers makes it impossible for the N(C)-ASH gel to completely wrap the fibers, resulting in hollow defect areas. In addition, the fluidity of the slurry decreases during stirring, and the bubbles in the slurry are not easily broken by vibration, which increases the porosity and reduces the strength. The decrease in structural stability will also affect the overall shrinkage of the mortar.

[0106] 3.2 X-ray diffraction (XRD) analysis

[0107] Figure 3 The XRD patterns of the geopolymers prepared by using HPMC and CCCW in different dosages and the blank geopolymers are shown in FIG. Figure 3 It can be clearly found that there is a significant diffusion peak at a diffraction angle of 25° to 30°, which is the characteristic peak of the amorphous phase of N(C)-ASH gel. Figure 3 It can be clearly seen that with the increase of HPMC dosage, the characteristic peak of amorphous SiO2 in the original kaolin with a diffraction angle of about 22° gradually disappears, and the diffusion peak of N(C)-ASH gel gradually becomes prominent, indicating that the addition of HPMC

[0108] It will promote the formation of more N(C)-ASH gel in geopolymer mortar. This is because water does not react directly in geopolymer, but provides a medium and space for geopolymer reaction. The addition of HPMC improves the water retention of mortar, delays the rate of water escape, and allows more sufficient reaction time between geopolymer precursor and activator. However, this does not bring about an improvement in the mechanical strength of geopolymer mortar. This may be related to the introduction of more pores inside after the addition of HPMC.

[0109] By comparing the XRD patterns after the addition of CCCW, it can be found that the diffusion peak at the diffraction angle of 25°~30° is also slightly enhanced. This is because the active substances such as tricalcium silicate and active magnesium in CCCW generate CSH gel MASH gel under alkaline conditions.

[0110] 3.3 Fourier transform infrared spectroscopy (FT-IR) analysis

[0111] Figure 4 The infrared spectra of the samples doped with HPMC, CCCW and blank samples of the present invention are located at 3470.16 cm -1 and 1658cm -1The absorption peak of 3470.16cm is due to the stretching vibration of the OH bond and the bending vibration of HOH in the geopolymer. It can be clearly observed from the figure that after the addition of HPMC and CCCW, the absorption peak originally located at 3470.16cm -1 The absorption peak of 1028.36cm-1 becomes wider and gradually shifts to the low frequency region, proving that more crystal water is generated. -1 The absorption peaks on the left and right correspond to the Si-O-Si(Al) bonds in the silicon (aluminum) oxygen tetrahedron in the geopolymer, which are characteristic peaks of the typical silicate glass phase. After the addition of HPMC, the peak intensity decreases and shifts to the low-frequency region. This is because the increase in the Al-0 bonds with longer bond lengths in the geopolymer causes the overall bond energy to decrease. This means that more Si ions in the four-coordinated SiO4 are replaced by Al ions in the geopolymer reaction, indicating an increase in the degree of reaction.

[0112] 3.4 Thermogravimetric (TG-DTG) analysis

[0113] like Figure 6 As shown, Figure 6 The TG-DTG spectrum comparison diagram of the sample doped with CCCW and the blank sample of the present invention. In order to further explore the products in the pore structure of geopolymer mortar after adding CCCW, the sample after curing for 28 days after adding CCCW was analyzed by thermogravimetric (TG-DTG). Figure 6 It can be seen that the sample mainly loses weight in the range of 120-150°C, which is caused by the loss of crystal water of ettringite and N(C, M)-ASH gel. After adding CCCW, the sample loses more mass in this range compared with the blank group. This is because the ettringite and hydrated aluminum (magnesium) calcium silicate produced after the hydration of CCCW carry more crystal water, which is consistent with the previous infrared spectrum analysis.

[0114] 3.5 Mercury Intrusion Porosimetry (MIP) Porosity Test Analysis

[0115] Table 6 shows the mercury injection results of samples at different dosages. It can be seen from Table 6 that as the HPMC dosage increases, the total porosity of the sample will also increase. The pores in the concrete are divided into four categories according to the pore size: those less than 20nm are harmless pores, those between 20 and 100nm are less harmful pores, those between 100 and 200nm are harmful pores, and those greater than 200nm are more harmful pores. Figure 5 It can be seen that after adding 0.2% HPMC, the porosity increases slightly, and the increased pore size is around 8140nm. After adding 0.6% HPMC, the total porosity increases dramatically, and the increased pore size is mostly around 26200nm. This shows that adding MPMC will increase the total porosity, and it is a multi-damaged pore.

[0116] Table 6

[0117]

[0118] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A multi-parameter performance prediction method for geopolymer-based composite repair mortar based on response surface theory, comprising the following steps: (1) Determine the basic formula of geopolymer-based composite repair mortar, including the configuration of aggregate, geopolymer precursor and alkaline activator; (2) Using single factor experiments to determine the setting range of each variable and designing several groups of mix ratios of geopolymer-based composite repair mortars; (3) mixing and pouring the geopolymer-based composite repair mortar, and obtaining the response value by means of an experimental method; (4) Fitting a quadratic model to the main variable and the response value to obtain a quadratic polynomial regression equation; (5) Analyze the fitting results and verify their significance; (6) Set the expected value and use the response surface equation to solve the optimal mix ratio; (7) Conduct an experiment using the method of step (3) to verify the accuracy of the optimal solution of step (6).

2. The multi-parameter performance prediction method of geopolymer-based composite repair mortar based on response surface theory according to claim 1 is characterized in that: In step (1), the type and particle size of aggregate, the type and fineness of geopolymer precursor, and the type, modulus and concentration of alkaline activator are used as preset parameters.

3. The multi-parameter performance prediction method of geopolymer-based composite repair mortar based on response surface theory according to claim 1 is characterized in that: In step (2), the variables include the type and dosage of polypropylene fiber PPF, cement-based infiltrative crystallization material CCCW, and hydroxypropyl methylcellulose HPMC.

4. The multi-parameter performance prediction method of geopolymer-based composite repair mortar based on response surface theory according to claim 1 is characterized in that: In step (3), the molding method of the geopolymer composite repair mortar includes first dry-mixing the geopolymer precursor and the main variable for a preset time, then adding an alkaline activator and stirring for a preset time to obtain a slurry, pouring the mixture slurry into a mold, waiting for a preset time to demold, and standard curing until a preset time. The test method adopts a compression test, a flexural test and an expansion and contraction test.

5. The multi-parameter performance prediction method of geopolymer-based composite repair mortar based on response surface theory according to claim 1 is characterized in that: In step (4), the measured data are fitted with a quadratic model using the response surface method to obtain quadratic polynomial regression equations for compressive strength Y1, fluidity Y2, and 7d shrinkage value Y3, as shown in equations (1) to (3): Y1=75.05-0.9675*A-1.16*B+0.6437*C-0.5025*AB+0.2075*AC-0.32*BC+0.1835*A2-1.88*B2-1.95*C2(1) Y2=194.64-2.9*A+1.2*B-14.8*C-1.25*AB+4.85*AC+1.5*BC-1.95*A2+3.55*B2+4.31*C2(2) Y3=127-16.63*A-2.75*B-10.88*C-24.75*AB+9.5*AC+2.75*BC+47.25A2+22B2-21.25*C2(3).

6. The multi-parameter performance prediction method of geopolymer-based composite repair mortar based on response surface theory according to claim 1 is characterized in that: In step (6), the expected values ​​and the optimized dosages of polypropylene fiber PPF, cement-based permeable crystallization material CCCW, and hydroxypropyl methylcellulose HPMC are set; in step (7), the verification method, verification value, and error adopted for the optimal mix ratio.

7. The method for preparing the geopolymer-based composite repair mortar according to claim 6, characterized in that: In step (7), the compressive and flexural strength tests are performed on the test blocks after the predetermined curing time to obtain the response values, which are input into the Design Expert software platform together with the expansion and contraction response values ​​for response surface analysis. The interaction and significance level of each variable in the response value are analyzed using a significance test, and a P value of <0.05 is considered significant. The global expectation of 28d compressive strength and fluidity being high and shrinkage being low is set, and the mix ratio with the best comprehensive performance is solved and verified by the above experiment. The errors are compared. If the error is less than 5%, the predicted value is considered to be consistent with the actual value. Otherwise, the above steps are repeated.

8. The multi-parameter performance prediction method of geopolymer-based composite repair mortar based on response surface theory according to claim 1 is characterized in that: In step (1), the geopolymer-based composite repair mortar comprises the following components in parts by weight: The alkaline activator is a mixture of sodium silicate Na2SiO3 and sodium hydroxide NaOH, wherein the modulus of the sodium silicate is 2.3, the concentration is 43.5%, the mass fraction ratio of SiO2 is 29.99%, the mass fraction ratio of Na2O is 13.75%, and the purity of the sodium hydroxide is 99%. By mass, 104 parts of sodium hydroxide are dissolved in 250 parts of water to prepare a sodium hydroxide solution, and after the solution is cooled, it is mixed with 650 parts of sodium silicate, fully stirred and left to stand for 12 hours for use.

9. The multi-parameter performance prediction method of geopolymer-based composite repair mortar based on response surface theory according to claim 8, characterized in that: In step (1), the method for preparing the geopolymer-based composite repair mortar comprises the following steps: Step 1: Use 800-mesh metakaolin as a precursor, add 650 parts of metakaolin by weight to the polypropylene PP fiber, cement-based infiltration crystallization material and hydroxypropyl methylcellulose in the precursor according to claim 8, and pre-mix for 3 minutes; Step 2: Add 500 parts of the prepared and aged alkaline activator to the geopolymer precursor and stir at low speed for 2 minutes, then add 1350 parts of Chinese IOS standard sand and stir at high speed for 3 minutes to obtain a slurry; Step 3: Load the slurry into an expansion and contraction instrument for testing or into a 160mm*40mm*40mm plastic test mold, and vibrate it for 2 minutes using a cement mortar vibrator with a vibration frequency of 1Hz. Scrape it until it is still and wait for 24 hours before demolding. Transfer it to a standard curing room for curing for a predetermined time to obtain a geopolymer-based composite repair mortar.

10. Geopolymer-based composite repair mortar prepared by the method of claim 9.

Citation Information

Cited By

  • Multi-objective optimization method for strain hardening alkali-activated concrete material

    CN120412844A

  • Method for determining influence of waste incineration bottom ash on mortar performance based on hyperspectral data

    CN121364160A