Corrosion-resistant low-voltage aerial insulated cable
By using a composite insulation and sheath layer of boron nitride and chitosan-modified illite powder in the cable, the strength and corrosion resistance of overhead insulated cables in corrosive environments have been solved, achieving a significant improvement in the cable's strength and corrosion resistance.
Patent Information
- Application Number
- CN202411236006.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing overhead insulated cables are prone to corrosion and damage in humid and highly corrosive environments, resulting in poor strength, short service life, and high maintenance frequency and cost.
Corrosion-resistant low-voltage overhead insulated cables are prepared by extrusion molding using an insulation layer and a sheath layer made of boron nitride and chitosan-modified illite powder, thereby improving the strength and corrosion resistance of the cables.
It significantly improves the tensile strength and corrosion resistance of cables, reduces maintenance frequency and costs, and extends the service life of cables.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of power cables, and in particular to a corrosion-resistant low-voltage overhead insulated cable. Background Art
[0002] In the field of modern power transmission, overhead insulated cables are widely used due to their unique advantages. However, for some special environments, such as humid and highly corrosive areas, facing the erosion of various corrosive media, such as acid, alkali, salt, etc., higher requirements are placed on overhead insulated cables. During the overhead laying process, cables with poor strength are also easily damaged by natural external forces such as wind, rain, ice and snow, as well as artificial external forces, which greatly reduces the service life of the cable and increases the frequency and cost of replacement and maintenance. Therefore, it is necessary to obtain a low-voltage overhead insulated cable with excellent corrosion resistance and high strength to meet the needs of power transmission in special environments, improve power supply reliability, and promote the development of the power industry. Summary of the invention
[0003] The invention provides a corrosion-resistant low-voltage overhead insulated cable, which solves the problem of poor strength and corrosion resistance of the overhead insulated cable in the related art.
[0004] The technical solution of the present invention is as follows: The present invention provides a corrosion-resistant low-voltage overhead insulated cable, comprising a conductor and an insulating layer, an armor layer, and a sheath layer sequentially arranged outside the conductor; The insulating layer comprises the following components in parts by weight: 70-80 parts of polyethylene, 20-30 parts of polyvinyl chloride, 5-10 parts of filler, 3-5 parts of compatibilizer, 3-5 parts of cross-linking agent, 1-2 parts of plasticizer, and 1-3 parts of antioxidant; The sheath layer comprises the following components in parts by weight: 100 parts of polyvinyl chloride, 8 to 16 parts of filler, 1 to 2 parts of plasticizer, and 1 to 3 parts of antioxidant; The fillers of the insulating layer and the sheath layer independently include boron nitride and modified illite powder; The modified illite powder is obtained by modifying the illite powder with chitosan.
[0005] As a further technical solution, the mass ratio of the boron nitride to the modified illite powder is 1:4-9.
[0006] In the present invention, the strength and corrosion resistance of the cable are further improved by limiting the mass ratio of boron nitride to modified illite powder to 1:4-9.
[0007] As a further technical solution, the method for preparing the modified illite powder comprises the following steps: The chitosan and illite powder are mixed and dried to obtain modified illite powder.
[0008] As a further technical solution, the mass ratio of the chitosan to the illite powder is 2-3:10.
[0009] As a further technical solution, the mixing is wet mixing, the solvent of the wet mixing is a dilute acetic acid solution, and the time is 50 to 80 minutes.
[0010] As a further technical solution, the modified illite powder is obtained by sequentially modifying the illite powder with chitosan and hydroxy acrylic resin.
[0011] In the present invention, illite powder is modified by chitosan and hydroxy acrylic resin in sequence, thereby further improving the strength and corrosion resistance of the cable.
[0012] As a further technical solution, the preparation method of the modified illite powder comprises the following steps: mixing the chitosan and illite powder, drying them, and then mixing them with the hydroxy acrylic resin to obtain the modified illite powder.
[0013] As a further technical solution, the mass ratio of the chitosan, illite powder and hydroxy acrylic resin is 3:10:1-2.
[0014] As a further technical solution, the plasticizer includes phthalate plasticizer and / or terephthalate plasticizer; the antioxidant includes amine antioxidant and / or triester phosphite antioxidant; the compatibilizer includes maleic anhydride grafted polyethylene; and the crosslinking agent is peroxide.
[0015] The present invention also provides a method for preparing the corrosion-resistant low-voltage overhead insulated cable, comprising the following steps: After the components of the insulating layer and the sheath layer are mixed respectively, the insulating layer is extruded between the conductor and the armor layer, and the sheath layer is extruded outside the armor layer, and the molding is performed to obtain a corrosion-resistant low-voltage overhead insulated cable.
[0016] The working principle and beneficial effects of the present invention are: In the present invention, the structure of the corrosion-resistant low-voltage overhead insulated cable includes a conductor and an insulating layer, an armor layer, and a sheath layer which are sequentially arranged outside the conductor. Boron nitride and chitosan-modified illite powder are added to the insulating layer and the sheath layer for compounding, thereby significantly improving the strength and corrosion resistance of the cable. DETAILED DESCRIPTION
[0017] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] In the following examples and comparative examples, the model of polyethylene is T5070; the model of polyvinyl chloride is C-15; and the model of maleic anhydride grafted polyethylene is M623XF.
[0019] Example 1 Corrosion-resistant low-voltage overhead insulated cable, comprising a conductor and an insulating layer, an armor layer and a sheath layer arranged outside the conductor in sequence; The insulating layer includes the following components in parts by weight: 70 parts of polyethylene, 20 parts of polyvinyl chloride, 5 parts of filler, 3 parts of maleic anhydride grafted polyethylene, 3 parts of dibenzoyl peroxide, 1 part of dioctyl phthalate, and 1 part of antioxidant D; The sheath layer comprises the following components in parts by weight: 100 parts of polyvinyl chloride, 8 parts of filler, 1 part of dioctyl phthalate, and 1 part of antioxidant D; The filler is boron nitride and modified illite powder in a mass ratio of 1:3; The modified illite powder is obtained by modifying the illite powder with chitosan. The preparation method of the modified illite powder comprises the following steps: 2 g of chitosan, 30 mL of dilute acetic acid solution and 10 g of illite powder were mixed for 80 min and dried to obtain modified illite powder; The preparation method of the corrosion-resistant low-voltage overhead insulated cable comprises the following steps: After the components of the insulating layer and the sheath layer are mixed respectively, the insulating layer is extruded between the conductor and the armor layer, and the sheath layer is extruded outside the armor layer, and the corrosion-resistant low-voltage overhead insulated cable is obtained.
[0020] Example 2 Corrosion-resistant low-voltage overhead insulated cable, comprising a conductor and an insulating layer, an armor layer and a sheath layer arranged outside the conductor in sequence; The insulating layer comprises the following components in parts by weight: 75 parts of polyethylene, 25 parts of polyvinyl chloride, 8 parts of filler, 4 parts of maleic anhydride grafted polyethylene, 4 parts of dibenzoyl peroxide, 1-21.5 parts of dioctyl phthalate, and 2 parts of antioxidant D; The sheath layer comprises the following components in parts by weight: 100 parts of polyvinyl chloride, 11 parts of filler, 1 part of dioctyl phthalate, and 2 parts of antioxidant D; The filler is boron nitride and modified illite powder in a mass ratio of 1:3; The modified illite powder is obtained by modifying the illite powder with chitosan. The preparation method of the modified illite powder comprises the following steps: 1.5 g of chitosan, 30 mL of dilute acetic acid solution and 10 g of illite powder were mixed for 70 min and dried to obtain modified illite powder; The preparation method of the corrosion-resistant low-voltage overhead insulated cable comprises the following steps: After the components of the insulating layer and the sheath layer are mixed respectively, the insulating layer is extruded between the conductor and the armor layer, and the sheath layer is extruded outside the armor layer, and the corrosion-resistant low-voltage overhead insulated cable is obtained.
[0021] Example 3 Corrosion-resistant low-voltage overhead insulated cable, comprising a conductor and an insulating layer, an armor layer and a sheath layer arranged outside the conductor in sequence; The insulating layer includes the following components in parts by weight: 80 parts of polyethylene, 30 parts of polyvinyl chloride, 10 parts of filler, 5 parts of maleic anhydride grafted polyethylene, 5 parts of dibenzoyl peroxide, 2 parts of dioctyl phthalate, and 3 parts of antioxidant D; The sheath layer comprises the following components in parts by weight: 100 parts of polyvinyl chloride, 16 parts of filler, 2 parts of dioctyl phthalate, and 3 parts of antioxidant D; The filler is boron nitride and modified illite powder in a mass ratio of 1:3; The modified illite powder is obtained by modifying the illite powder with chitosan. The preparation method of the modified illite powder comprises the following steps: 3 g of chitosan, 30 mL of dilute acetic acid solution and 10 g of illite powder were mixed for 50 min and dried to obtain modified illite powder; The preparation method of the corrosion-resistant low-voltage overhead insulated cable comprises the following steps: After the components of the insulating layer and the sheath layer are mixed respectively, the insulating layer is extruded between the conductor and the armor layer, and the sheath layer is extruded outside the armor layer, and the corrosion-resistant low-voltage overhead insulated cable is obtained.
[0022] Example 4 The only difference between this embodiment and embodiment 3 is that the filler is boron nitride and modified illite powder in a mass ratio of 1:10.
[0023] Example 5 The only difference between this embodiment and embodiment 3 is that the filler is boron nitride and modified illite powder in a mass ratio of 1:4.
[0024] Example 6 The only difference between this embodiment and embodiment 3 is that the filler is boron nitride and modified illite powder in a mass ratio of 1:9.
[0025] Example 7 The difference between this embodiment and embodiment 6 is that the modified illite powder is obtained by modifying the illite powder with hydroxy acrylic resin, and the preparation method of the modified illite powder comprises the following steps: 0.5 g of hydroxy acrylic resin, 30 mL of water and 10 g of illite powder were mixed for 50 minutes and dried to obtain modified illite powder.
[0026] Example 8 The difference between this embodiment and embodiment 6 is that the modified illite powder is obtained by sequentially modifying the illite powder with hydroxy acrylic resin and chitosan, and the preparation method of the modified illite powder comprises the following steps: 3 g of chitosan, 30 mL of dilute acetic acid solution and 10 g of illite powder were mixed for 50 minutes, dried, mixed with 0.5 g of hydroxy acrylic resin and 10 mL of water, and dried to obtain modified illite powder.
[0027] Example 9 The difference between this embodiment and embodiment 6 is that the modified illite powder is obtained by sequentially modifying the illite powder with hydroxy acrylic resin and chitosan, and the preparation method of the modified illite powder comprises the following steps: 3 g of chitosan, 30 mL of dilute acetic acid solution and 10 g of illite powder were mixed for 50 minutes, dried, mixed with 3 g of hydroxy acrylic resin and 10 mL of water, and dried to obtain modified illite powder.
[0028] Example 10 The difference between this embodiment and embodiment 6 is that the modified illite powder is obtained by sequentially modifying the illite powder with hydroxy acrylic resin and chitosan, and the preparation method of the modified illite powder comprises the following steps: 3 g of chitosan, 30 mL of dilute acetic acid solution and 10 g of illite powder were mixed for 50 minutes, dried, mixed with 1 g of hydroxy acrylic resin and 10 mL of water, and dried to obtain modified illite powder.
[0029] Embodiment 11 The difference between this embodiment and embodiment 6 is that the modified illite powder is obtained by sequentially modifying the illite powder with hydroxy acrylic resin and chitosan, and the preparation method of the modified illite powder comprises the following steps: 3 g of chitosan, 30 mL of dilute acetic acid solution and 10 g of illite powder were mixed for 50 minutes, dried, mixed with 2 g of hydroxy acrylic resin and 10 mL of water, and dried to obtain modified illite powder.
[0030] Comparative Example 1 The only difference between this comparative example and Example 3 is that the filler is boron nitride.
[0031] Comparative Example 2 The only difference between this comparative example and Example 3 is that the filler is modified illite powder.
[0032] Comparative Example 3 The difference between this comparative example and Example 3 is that the filler is boron nitride and illite powder in a mass ratio of 1:3.
[0033] After the sheath layer of the corrosion-resistant low-voltage overhead insulated cable prepared in Examples 1 to 11 and Comparative Examples 1 to 3 was subjected to an acid immersion test (immersed in 20wt% hydrochloric acid for 30 days), the tensile strength before and after acid immersion was tested in accordance with standard GB / T 12706.1-2020 "Extruded insulated power cables and accessories with rated voltage of 1 kV (Um=1.2 kV) to 35 kV (Um=40.5 kV) Part 1: Cables with rated voltage of 1 kV (Um=1.2kV) and 3 kV (Um=3.6 kV)", and the tensile strength retention rate was calculated. The test results are shown in Table 1 below.
[0034] Table 1 Test results of sheath performance of corrosion-resistant low-voltage overhead insulated cable
[0035] Compared with Comparative Examples 1 to 3, the sheath layers of the corrosion-resistant low-voltage overhead insulated cables prepared in Examples 1 to 11 have higher tensile strength and better tensile strength retention, indicating that the strength and corrosion resistance of the cable are significantly improved by adding boron nitride and chitosan-modified illite powder to the sheath layer for compounding.
[0036] Compared with Examples 3 to 4, the tensile strength of the sheath layer of the corrosion-resistant low-voltage overhead insulated cable prepared in Examples 5 to 6 is higher and the tensile strength retention rate is better, indicating that limiting the mass ratio of boron nitride to modified illite powder to 1:4 to 9 further improves the strength and corrosion resistance of the cable.
[0037] Compared with Examples 6 to 7, the tensile strength of the sheath layer of the corrosion-resistant low-voltage overhead insulated cable prepared in Examples 8 to 11 is higher, and the tensile strength retention rate is better, indicating that the illite powder is modified by chitosan and hydroxy acrylic resin in sequence, and the strength and corrosion resistance of the cable are further improved; compared with Examples 8 to 9, the tensile strength of the sheath layer of the corrosion-resistant low-voltage overhead insulated cable prepared in Examples 10 to 11 is higher, and the tensile strength retention rate is better, indicating that the illite powder is modified by chitosan and hydroxy acrylic resin in sequence, and the strength and corrosion resistance of the cable are further improved.
[0038] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A corrosion-resistant low-voltage overhead insulated cable, characterized in that: It comprises a conductor and an insulating layer, an armor layer and a sheath layer arranged in sequence outside the conductor; The insulating layer comprises the following components in parts by weight: 70-80 parts of polyethylene, 20-30 parts of polyvinyl chloride, 5-10 parts of filler, 3-5 parts of compatibilizer, 3-5 parts of cross-linking agent, 1-2 parts of plasticizer, and 1-3 parts of antioxidant; The sheath layer comprises the following components in parts by weight: 100 parts of polyvinyl chloride, 8 to 16 parts of filler, 1 to 2 parts of plasticizer, and 1 to 3 parts of antioxidant; The fillers of the insulating layer and the sheath layer independently include boron nitride and modified illite powder; The modified illite powder is obtained by modifying the illite powder with chitosan.
2. A corrosion-resistant low-voltage overhead insulated cable according to claim 1, characterized in that: The mass ratio of the boron nitride to the modified illite powder is 1:4-9.
3. A corrosion-resistant low-voltage overhead insulated cable according to claim 1, characterized in that: The preparation method of the modified illite powder comprises the following steps: The chitosan and illite powder are mixed and dried to obtain modified illite powder.
4. A corrosion-resistant low-voltage overhead insulated cable according to claim 3, characterized in that: The mass ratio of the chitosan to the illite powder is 2-3:
10.
5. A corrosion-resistant low-voltage overhead insulated cable according to claim 3, characterized in that: The mixing is wet mixing, the solvent of the wet mixing is a dilute acetic acid solution, and the time is 50 to 80 minutes.
6. A corrosion-resistant low-voltage overhead insulated cable according to claim 1, characterized in that: The modified illite powder is obtained by sequentially modifying the illite powder with chitosan and hydroxy acrylic resin.
7. A corrosion-resistant low-voltage overhead insulated cable according to claim 6, characterized in that: The preparation method of the modified illite powder comprises the following steps: mixing the chitosan and the illite powder, drying them, and then mixing them with the hydroxy acrylic resin to obtain the modified illite powder.
8. A corrosion-resistant low-voltage overhead insulated cable according to claim 7, characterized in that: The mass ratio of the chitosan illite powder to the hydroxy acrylic resin is 3:10:1-2.
9. The corrosion-resistant low-voltage overhead insulated cable according to claim 1, characterized in that: The plasticizer includes phthalate plasticizer and / or terephthalate plasticizer; the antioxidant includes amine antioxidant and / or triester phosphite antioxidant; the compatibilizer includes maleic anhydride grafted polyethylene; and the crosslinking agent is peroxide.
10. A method for preparing a corrosion-resistant low-voltage overhead insulated cable according to any one of claims 1 to 9, characterized in that: The following steps are involved: After the components of the insulating layer and the sheath layer are mixed respectively, the insulating layer is extruded between the conductor and the armor layer, and the sheath layer is extruded outside the armor layer, and the molding is performed to obtain a corrosion-resistant low-voltage overhead insulated cable.
Citation Information
Cited By
Anti-freezing power cable
CN119331321A
An anti-freeze power cable
CN119331321B