Preparation method and application of Ni3Al superconducting wire doped with zinc iodide
By doping zinc iodide in the Nb/Al precursor and performing specific heat treatment, the problem of poor performance of Nb3Al superconducting materials in the prior art was solved, and a niobium trialuminum superconducting with high superconducting transition temperature and excellent performance was prepared. Wire material meets the current carrying capacity requirements of high-field superconducting magnets.
Patent Information
- Application Number
- CN202411237232.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-04
AI Technical Summary
It is difficult to prepare Nb3Al superconducting materials with Nb:Al=3:1 that meets the stoichiometric ratio, resulting in poor superconducting performance and cannot meet the current carrying capacity requirements of high-field superconducting magnets.
By doping zinc iodide in the Nb/Al precursor, the decomposition reaction of zinc iodide is used to generate Nb with fine particle size, combined with RHQ treatment and low temperature annealing, a niobium trialuminum superconducting wire that meets the stoichiometric ratio is prepared, which improves the Superconducting performance.
The prepared niobium trialuminum superconducting wire has high superconducting transition temperature and excellent superconducting performance. The critical current density reaches 3.67×104A/cm2 at 8T, meeting the needs of high-field superconducting magnets.
Smart Images

Figure CN119049795A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of superconducting materials, and in particular to a preparation method and application of a zinc iodide-doped niobium-aluminum superconducting wire. Background Art
[0002] Nuclear fusion power generation has the advantages of being more environmentally friendly, more efficient, and more stable. Magnetic confinement nuclear fusion technology is one of the main technologies for achieving controlled nuclear fusion reactions. Currently, the main material for large-size, strong magnetic field, and large current magnetic confinement superconducting coils is Nb3Sn superconductor. Large currents will generate huge Lorentz forces in strong magnetic fields, which will attenuate the current carrying capacity of Nb3Sn superconducting wires, so higher-field superconducting magnets are needed. Compared with Nb3Sn, Nb3Al superconducting materials have a higher superconducting transition temperature (T c ), upper critical field (B irr ) and far superior stress-strain resistance. When subjected to the same 0.4% tensile strain, the current carrying capacity of Nb3Al superconducting wire decays by about 10%, while that of Nb3Sn decays by about 40%. The use of Nb3Al superconductors to prepare large superconducting magnets for nuclear fusion devices can ensure that the service performance of the magnets is consistent with the design. Therefore, Nb3Al is regarded as an ideal material to replace Nb3Sn, making the characteristics and preparation process of Nb3Al superconductors widely studied.
[0003] High-performance Nb3Al superconductors are inseparable from the stoichiometric Nb / Al distribution, so it is critical to prepare a stoichiometric ratio, that is, Nb:Al=3:1 (molar ratio). In the preparation process of Nb3Al superconductors, doping with other elements is an effective method to improve the superconducting properties of Nb3Al. The preparation of Nb3Al superconducting wires mainly includes two steps: precursor wire and heat treatment phase formation. The preparation of precursor wires mainly includes: powder tube method, casing method, winding method, etc. Heat treatment phase formation mainly includes low-temperature heat treatment and high-temperature heat treatment. The superconducting properties of Nb3Al are very sensitive to the heat treatment temperature. The performance of Nb3Al superconducting wires prepared below 1800℃ is very poor because the generated Nb3Al superconducting phase deviates seriously from the stoichiometric ratio (that is, Nb:Al=3:1). The phase formation temperature of Nb3Al that meets the stoichiometric ratio is between 1940℃ and 2060℃, and its superconducting transition temperature (T c ) exceeds 18K. However, Nb3Al prepared by the prior art generally deviates from the stoichiometric ratio, that is, the purity is low and the superconducting performance is poor. Therefore, it is an urgent problem to provide a Nb3Al superconductor with a stoichiometric ratio close to Nb:Al=3:1 (molar ratio) and good superconducting performance. In view of the above problems, the present invention proposes a preparation method and application of a zinc iodide-doped niobium trialuminum superconducting wire. Summary of the invention
[0004] The purpose of the present invention is to provide a preparation method and application of a zinc iodide-doped niobium-aluminum superconducting wire. The prepared niobium-aluminum superconducting wire is a highly uniform A15 phase Nb3Al superconducting wire, the molar ratio of Nb:Al is close to the stoichiometric ratio of 3:1, the superconducting phase is purer, the critical current density is high, and the superconducting performance is excellent.
[0005] To achieve the above object, the present invention provides a method for preparing a zinc iodide-doped niobium-aluminum superconducting wire, which specifically comprises the following steps:
[0006] (1) In an inert atmosphere, zinc iodide powder, Nb powder and Al powder are uniformly mixed to obtain a mixed powder; the mixed powder is molded to obtain a zinc iodide-doped Nb / Al precursor wire, and then the zinc iodide-doped Nb / Al precursor wire is placed in a tube furnace for heating and then kept warm;
[0007] (2) subjecting the zinc iodide-doped Nb / Al precursor wire obtained in step (1) to RHQ treatment to obtain a supersaturated solid solution Nb(Al) ss Wire;
[0008] (3) The supersaturated solid solution Nb(Al) obtained in step (2) ss The wire is subjected to low temperature annealing to obtain a zinc iodide-doped niobium-aluminum superconducting wire.
[0009] Preferably, in step (1), the molar ratio of Nb powder to Al powder is 74:26, wherein the average particle size of Nb powder is 5 to 45 μm, and the average particle size of Al powder is 25 to 45 μm.
[0010] Preferably, in step (1), the mass percentage of zinc iodide in the mixed powder is 0.1% to 3%.
[0011] Preferably, in step (1), the mass percentage of zinc iodide in the mixed powder is 0.5-1.5%.
[0012] Preferably, in step (1), the heating temperature is 1150° C. and the temperature is kept for 30 minutes.
[0013] Preferably, in the step (1), the specific operation of the molding process is to load the mixed powder into a Nb tube and fill it tightly to obtain a Nb tube filled with powder, and then put the Nb tube filled with powder into a rotary forging machine for processing to obtain a Nb / Al precursor wire doped with zinc iodide.
[0014] Preferably, in the step (2), the specific operation of the RHQ treatment is to load a direct current of 100 to 220 A to the Nb / Al precursor wire doped with zinc iodide, heat the Nb / Al precursor wire doped with zinc iodide to 2000° C. within 2 to 10 seconds, and then quench it to 50° C.
[0015] Preferably, in the step (3), the temperature of the low-temperature annealing is 790-820° C., and the time of the low-temperature annealing is 8-11 hours.
[0016] The present invention also provides a zinc iodide-doped niobium-aluminum superconducting wire prepared by the above preparation method.
[0017] The present invention also provides the use of the prepared zinc iodide-doped niobium trialuminum superconducting wire in a superconducting magnet.
[0018] The present invention places a zinc iodide-doped Nb / Al precursor wire in a tubular furnace. Under the condition of 1150° C., the zinc iodide is decomposed into iodine and fine-grained zinc. Nb reacts with the iodine and decomposes while reacting to generate Nb with a smaller particle size. The Nb with a smaller particle size reacts more fully with Al during RHQ treatment, while the Zn with a smaller particle size serves as a pinning center to improve the superconducting performance of the wire.
[0019] The preparation method provided by the present invention comprises the following steps: zinc iodide is doped into Nb during the preparation process, that is, a zinc iodide-doped Nb / Al precursor wire is first prepared, ZnI2 is decomposed into I2 and Zn at 1150°C, a chemical reaction Nb+2I2→NbI4 occurs between I and Nb at about 1150°C, and a decomposition reaction occurs while a chemical reaction occurs during the process to form Nb, and the Nb generated by the decomposition reaction achieves the purpose of refining Nb, so that the particle size of Nb reacting with Al becomes smaller, and in the RHQ treatment (i.e., rapid heating and cooling treatment) process, Nb and Al react more fully, and a purer Nb3Al superconducting phase that is more in line with the stoichiometric ratio of 76:24 is generated, thereby improving the superconducting performance of the prepared niobium-aluminum superconducting wire, and obtaining a zinc iodide-doped niobium-aluminum superconducting wire with a high superconducting transition temperature and excellent superconducting performance. The stoichiometric ratio of Nb to Al in the zinc iodide-doped niobium-aluminum superconducting wire prepared by the present invention is close to 74:26, and its critical current density J c (A / cm 2 ) reached 3.67×10 at 8T. 4 A / cm 2 , excellent superconducting performance.
[0020] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a scanning electron microscope image of the zinc iodide-doped niobium-aluminum superconducting wire prepared in Example 1 of the present invention;
[0022] Figure 2 The critical current density J of the ZnI-doped Nb3Al superconducting wire prepared in Example 1 of the present invention is c (A / cm2 ) changes with the magnetic field strength H(T). DETAILED DESCRIPTION
[0023] The present invention provides a method for preparing a zinc iodide-doped niobium-aluminum superconducting wire, which specifically comprises the following steps:
[0024] (1) In an inert atmosphere, zinc iodide powder, Nb powder and Al powder are uniformly mixed to obtain a mixed powder, and the mixed powder is molded to obtain a zinc iodide-doped Nb / Al precursor wire, and then the zinc iodide-doped Nb / Al precursor wire is placed in a tube furnace and heated at 1150° C., and then kept warm for 30 minutes. At this heating temperature, zinc iodide will decompose into iodine and fine zinc particles, and Nb will react with iodine, decomposing while reacting to generate Nb with a smaller particle size.
[0025] (2) subjecting the zinc iodide-doped Nb / Al precursor wire obtained in step (1) to RHQ treatment to obtain a supersaturated solid solution Nb(Al) ss Wire.
[0026] (3) the supersaturated solid solution Nb(Al) obtained in step (2) ss The wire is subjected to low temperature annealing to obtain a zinc iodide-doped niobium-aluminum superconducting wire.
[0027] In the present invention, the inert atmosphere is preferably argon.
[0028] In the present invention, the average particle size of Nb powder is preferably 5 to 45 μm, and the average particle size of Al powder is preferably 25 to 45 μm. The present invention controls the average particle size of Nb powder and Al powder within the above range to promote uniform mixing of the two and subsequent sufficient reaction, which is conducive to the generation of a purer Nb3Al superconducting phase that is more in line with the stoichiometric ratio of 76:24, thereby improving the superconducting performance of the prepared niobium-aluminum superconducting wire, and obtaining a zinc iodide-doped niobium-aluminum superconducting wire with a high superconducting transition temperature and excellent superconducting performance.
[0029] In the present invention, the molar ratio of the Nb powder to the Al powder is preferably 74: 26. The present invention controls the molar ratio of the Nb powder to the Al powder within the above range to avoid the loss of Al atoms during the preparation process, thereby facilitating the generation of a purer Nb3Al superconducting phase that is more in line with the stoichiometric ratio of 76:24, thereby improving the superconducting performance of the prepared niobium-aluminum superconducting wire.
[0030] In the present invention, the purity of the zinc iodide powder, Nb powder and Al powder is preferably >99.9% independently.
[0031] In the present invention, the mass percentage of zinc iodide in the mixed powder is preferably 0.1-3%, more preferably 0.5-1.5%. The present invention controls the mass percentage of zinc iodide in the mixed powder within the above range, and zinc iodide is decomposed into iodine and zinc at 1150°C. Since iodine is very easy to sublime, and the reaction of iodine and Nb is decomposition while reacting, too high a doping amount (greater than 1.5%) will cause zinc iodide to decompose when heated in a tubular furnace, and a large amount of iodine will sublimate and escape, resulting in more cracks on the surface of the wire, affecting the subsequent experimental process.
[0032] In the present invention, the molding process includes loading the mixed powder into a Nb tube and filling it tightly to obtain a Nb tube filled with powder, and then placing the Nb tube filled with powder into a rotary forging machine for processing to obtain a Nb / Al precursor wire doped with zinc iodide.
[0033] The present invention has no special restrictions on the method of placing the Nb tube filled with powder into the rotary forging machine for processing, and the Nb / Al precursor wire doped with zinc iodide can be obtained by adopting the technical solutions well known in the art.
[0034] In the present invention, the RHQ treatment preferably includes applying a direct current of 100 to 220 A to the zinc iodide-doped Nb / Al precursor wire, heating the zinc iodide-doped Nb / Al precursor wire to about 2000° C. within 2 to 10 seconds, and then rapidly quenching it to 50° C.
[0035] The present invention controls the DC current, heating temperature and rapid quenching temperature in the RHQ treatment within the above ranges, sets the current to 200A (according to the measured resistance of the wire and the experimental results, if the current is too low, the temperature cannot reach 2000°C, and if it is too high, the wire will explode), raises the temperature to about 2000°C (high temperatures above 1900°C will cause Nb / Al to react instantly to generate Nb3Al superconductors, and Nb3Al crystals will grow rapidly at high temperatures), and rapidly quenches the gallium liquid at about 50°C. Cold quenching can generate a bcc phase supersaturated solid solution Nb(Al)ss, and the generated A15 phase crystals are fine.
[0036] In the present invention, the temperature of the low-temperature annealing is preferably 790-820° C., more preferably 800° C. In the present invention, the time of the low-temperature annealing is preferably 8-11 hours, more preferably 10 hours.
[0037] The present invention also provides a zinc iodide-doped niobium trialuminum superconducting wire prepared by the preparation method described in the above technical solution, comprising a niobium trialuminum superconducting phase. The iodine content in the finally obtained wire is very low because the decomposed iodine escapes in large quantities after heating reaction in a tubular furnace.
[0038] The present invention also provides the use of the zinc iodide-doped niobium trialuminum superconducting wire described in the above technical solution in a superconducting magnet.
[0039] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Any other changes, modifications, substitutions, combinations, and simplifications made without violating the spirit and principle of the present invention should all be equivalent replacement methods and are included in the protection scope of the present invention. In addition, it should be understood that after reading the content of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application, and all belong to the scope of protection of the present invention.
[0040] Reference to "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The term "embodiment" appearing in various places in the specification does not necessarily refer to the same embodiment, nor does it particularly limit its independence or association with other embodiments. In principle, in the present application, as long as there is no technical contradiction or conflict, the various technical features mentioned in the embodiments can be combined in any way to form a corresponding implementable technical solution.
[0041] Unless otherwise defined, the technical terms used in this document have the same meanings as those generally understood by those skilled in the art to which this application belongs; the use of relevant terms in this document is only for describing specific embodiments and is not intended to limit this application.
[0042] Unless otherwise specified in the present invention, the reagents, instruments, equipment, etc. used are all reagents, instruments and equipment commonly used by technicians in this field, and are all conventional commercial products in this field and can be purchased through commercial channels.
[0043] Example 1
[0044] This embodiment provides a method for preparing a zinc iodide-doped niobium trialuminum superconducting wire, and the specific preparation steps are:
[0045] (1) Under argon protection, Nb powder (average particle size of 45 μm), Al powder (average particle size of 45 μm) and ZnI2 powder were weighed respectively, and mixed uniformly by planetary ball milling to obtain 13 g of mixed powder;
[0046] The mass percentage of the zinc iodide powder accounts for 1% of the mixed powder. To avoid the loss of Al atoms during the preparation process, the molar ratio of Nb powder to Al powder is 74:26. The purity of all powders is above 99.9%.
[0047] Under argon protection, the mixed powder is loaded into a Nb tube and filled tightly to obtain a Nb tube filled with powder, and the Nb tube filled with powder is put into a rotary forging machine for processing to obtain a zinc iodide-doped Nb / Al precursor wire with a diameter of 1.6 mm;
[0048] (2) cutting the zinc iodide-doped Nb / Al precursor wire obtained in step (1) into short wires of 10-15 cm in length, heating the short wires at 1050° C. for 30 minutes in a tube furnace, and then RHQ-loading them on a static heat treatment device, loading a direct current of 200 A, heating the zinc iodide-doped Nb / Al precursor wire to 2000° C. within <10 seconds, and then immediately quenching them rapidly to 50° C. in a room temperature liquid Ga pool to obtain a supersaturated solid solution Nb(Al)ss wire;
[0049] (3) the supersaturated solid solution Nb(Al) obtained in step (2) ss The wire was subjected to low temperature heat treatment at 800°C for 10 hours to obtain a zinc iodide-doped niobium-aluminum superconducting wire.
[0050] The microstructure and superconducting properties of the zinc iodide-doped niobium-aluminum superconducting wire prepared in this embodiment were tested.
[0051] 1. The niobium-aluminum superconducting wire doped with zinc iodide prepared in this embodiment was observed by scanning electron microscope, and the scanning electron micrograph was as follows: Figure 1 As shown. Figure 1 It can be seen that the stoichiometric ratio of Nb to Al in the ZnI-doped Nb3Al superconducting wire prepared in this embodiment is close to 74:26.
[0052] 2. The critical current density J of the zinc iodide-doped niobium-aluminum superconducting wire prepared in this embodiment was measured using the material comprehensive physical property measurement system PPMS-VSM method. c (A / cm 2 ) changes with the magnetic field H(T) as shown in the figure Figure 2 As shown. Figure 2 It can be seen that the critical current density J of the ZnI-doped Nb3Al superconducting wire prepared in this embodiment is c (A / cm 2 ) reached 3.67×10 at 8T. 4 A / cm 2 , excellent superconducting performance.
[0053] In summary, the stoichiometric ratio of Nb to Al in the ZnI-doped Nb3Al superconducting wire prepared by the present invention is close to 74:26, and its critical current density J at 4.2K is c (A / cm 2 ) reached 3.67×10 at 8T. 4 A / cm2 , the critical current density is higher than that of the pure sample, and the superconducting performance is excellent.
[0054] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing a zinc iodide-doped niobium trialuminum superconducting wire, characterized in that: The specific steps include: (1) In an inert atmosphere, zinc iodide powder, Nb powder and Al powder are uniformly mixed to obtain a mixed powder; the mixed powder is molded to obtain a zinc iodide-doped Nb / Al precursor wire, and then the zinc iodide-doped Nb / Al precursor wire is placed in a tube furnace for heating and then kept warm; (2) subjecting the zinc iodide-doped Nb / Al precursor wire obtained in step (1) to RHQ treatment to obtain a supersaturated solid solution Nb(Al) ss Wire; (3) The supersaturated solid solution Nb(Al) obtained in step (2) ss The wire is subjected to low temperature annealing to obtain a zinc iodide-doped niobium-aluminum superconducting wire.
2. The method for preparing a zinc iodide-doped niobium trialuminum superconducting wire according to claim 1, characterized in that: In the step (1), the molar ratio of Nb powder to Al powder is 74:26, wherein the average particle size of the Nb powder is 5 to 45 μm, and the average particle size of the Al powder is 25 to 45 μm.
3. The method for preparing a zinc iodide-doped niobium trialuminum superconducting wire according to claim 1, characterized in that: In the step (1), the mass percentage of zinc iodide in the mixed powder is 0.1% to 3%.
4. The method for preparing a zinc iodide-doped niobium trialuminum superconducting wire according to claim 3, characterized in that: In the step (1), the mass percentage of zinc iodide in the mixed powder is 0.5-1.5%.
5. The method for preparing a zinc iodide-doped niobium trialuminum superconducting wire according to claim 1, characterized in that: In the step (1), the heating temperature is 1150° C. and the temperature is kept at 1150° C. for 30 minutes.
6. The method for preparing a zinc iodide-doped niobium trialuminum superconducting wire according to claim 1, characterized in that: In the step (1), the specific operation of the molding process is to load the mixed powder into the Nb tube and fill it tightly to obtain the Nb tube filled with powder, and then put the Nb tube filled with powder into a rotary forging machine for processing to obtain the Nb / Al precursor wire doped with zinc iodide.
7. The method for preparing a zinc iodide-doped niobium trialuminum superconducting wire according to claim 1, characterized in that: In the step (2), the specific operation of the RHQ treatment is to load a direct current of 100 to 220 A to the zinc iodide-doped Nb / Al precursor wire, heat the zinc iodide-doped Nb / Al precursor wire to 2000° C. within 2 to 10 seconds, and then quench it to 50° C.
8. The method for preparing a zinc iodide-doped niobium trialuminum superconducting wire according to claim 1, characterized in that: In the step (3), the temperature of low temperature annealing is 790-820° C., and the time of low temperature annealing is 8-11 hours.
9. A zinc iodide-doped niobium trialuminum superconducting wire, characterized in that: The superconducting wire is prepared by the preparation method according to any one of claims 1 to 8.
10. The zinc iodide-doped niobium-aluminum superconducting wire according to claim 9, characterized in that: The superconducting wire is used in a superconducting magnet.
Citation Information
Patent Citations
Nanometer oxide-doped Nb3Al superconducting wire and preparation method thereof
CN115641997A
Nb3Al superconducting wire doped with elemental iodine and preparation method and application of Nb3Al superconducting wire
CN116884700A
Preparation method of Nb3Al superconducting wire with enhanced magnetic flux pinning capability
CN117577390A
Preparation method of niobium-aluminum-doped precursor wire