Ultracrystalline magnetic core and processing method thereof

By adopting the amorphous and nanocrystalline biphasic structure of ultramicrocrystalline magnetic core, combined with single-roll quenching method and vacuum muffle furnace heat treatment process, the problem of current transformer error control is solved, and efficient core performance improvement and simplified production is achieved. , significantly reduces cost and error.

CN119049843APending Publication Date: 2024-11-29SHENYANG UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411399663.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

During the manufacturing process of existing current transformers, error control is difficult to meet the national power grid standards, and the existing compensation methods are costly and inconvenient to implement.

Method used

The ultramicrocrystalline magnetic core is composed of amorphous and nanocrystalline biphasic structures, including iron, copper, niobium, silicon and boron elements. The strip is prepared by a single-roll quenching method, and the vacuum muffle furnace heat treatment and curing package are finally wound. Processing to achieve optimization of the magnetic core.

Benefits of technology

The induced potential and initial permeability of the ultramicrocrystalline magnetic core are improved, the core loss is reduced, the production process is simplified, and the cost is reduced. The product has excellent soft magnetic performance and significantly improved error control effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119049843A_ABST
    Figure CN119049843A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of ultracrystalline magnetic core preparation, in particular to an ultracrystalline magnetic core and a processing method thereof.The ultracrystalline magnetic core is composed of an amorphous and nanocrystalline two-phase structure, the average grain size is smaller than 25 nm, the ultracrystalline magnetic core is characterized by comprising an iron element, a copper element, a niobium element, a silicon element and a boron element, the molecular formula of the magnetic core is FeaCubNbcSidBe, according to the preparation method provided by the invention, the induced potential and the initial permeability of the ultracrystalline magnetic core can be simultaneously improved, the loss of the magnetic core is reduced, the production process is relatively simple and convenient, the cost is relatively low, industrialization is easy to realize, the produced product has excellent soft magnetic performance, the initial permeability can reach 11.84 million, the induced potential is increased by 23.8% under the condition of 50mA exciting current, and the initial permeability is increased by 23.8% under the condition of 50mA exciting current. Under the condition of 450mA excitation current, the induced potential is increased by 4.27%, and when the rated current percentage is 1% and 120%, the negative ratio difference is reduced by 0.05%, and the angular difference is reduced by 2.1 min and 3 min respectively.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ultra-microcrystalline magnetic core preparation, in particular to an ultra-microcrystalline magnetic core and a processing method thereof. Background Art

[0002] In the manufacturing process of current transformers, the error of current transformers is required to be low and within the error present value range of the national power grid. The existing method is to reduce the error by compensating the number of turns of the secondary winding or by compensating through an external circuit, which is costly and inconvenient.

[0003] In summary, it is necessary to propose an ultra-microcrystalline magnetic core and a processing method thereof to solve the above problems. Summary of the invention

[0004] The object of the present invention is to provide an ultra-fine crystal magnetic core and a processing method thereof to solve the problems raised in the above-mentioned background technology.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] An ultra-microcrystalline magnetic core, the magnetic core is composed of an amorphous and nanocrystalline dual-phase structure, the average grain size is less than 25nm, and includes iron, copper, niobium, silicon and boron. The molecular formula of the magnetic core is Fe a Cu b Nb c Si d B e .

[0007] Preferably, the magnetic core molecular formula is Fe a Cu b Nb c Si d B e Where a, b, c, d and e are the atomic ratios of the corresponding elements in the alloy, where:

[0008] 0.1≤b≤2;

[0009] 0.5≤c≤5;

[0010] 0.5≤d≤3;

[0011] 6≤e≤12.

[0012] Based on the above magnetic core, the present invention also proposes a method for preparing an ultra-microcrystalline magnetic core, comprising the following steps:

[0013] S1. The strip is prepared by a single-roller quenching method, and the ejected strip is divided into a free surface and a roller-attached surface;

[0014] S2. Heat treatment of the wound magnetic core is performed using a vacuum muffle furnace;

[0015] S3. Curing and packaging the heat-treated magnetic core;

[0016] S4. Wind the solidified and packaged magnetic core.

[0017] Preferably, the strip preparation in step S1 comprises the following steps:

[0018] S1.1. Prepare a strip with a thickness of 32-36um, a cooling roller speed of 1500-1650r / min, and a strip width of 25mm;

[0019] S1.2. Winding into a toroidal core with an inner diameter of 100 mm, an outer diameter of 123 ± 0.5 mm, a height of 25 mm, and a weight of 600 g;

[0020] S1.3. Use a semi-automatic winding device for manual winding and control the winding weight of the free side and the roller side.

[0021] Preferably, when the vacuum muffle furnace is used for heat treatment in step S2, the heating, insulation and cooling process of the wound magnetic core includes the following stages:

[0022] The room temperature was raised to 300°C in 70 minutes;

[0023] Heating from 300℃ to 400℃ takes 120 minutes, and keeping warm for 30 minutes;

[0024] Heating from 400℃ to 480℃ takes 90 minutes, and keeping warm for 90 minutes;

[0025] Heating from 480℃ to 555℃ takes 90 minutes and keeps warm for 60 minutes;

[0026] Finally, it is cooled to below 260℃ and taken out of the oven.

[0027] Preferably, the curing and packaging process of step S3 is as follows:

[0028] S3.1. Apply epoxy resin AB glue on one side and install it in the ball molding compound protective box;

[0029] S3.2. The dimensions of the protective box are inner diameter 95mm, outer diameter 130mm and height 30mm.

[0030] Preferably, the winding process of step S4 is:

[0031] S4.1. Use 1.45 mm and 0.51 mm copper wires in parallel to surround the core, with the wires evenly spaced.

[0032] S4.2. The number of turns of 0.51mm copper wire is one less than that of 1.45mm.

[0033] Compared with the prior art, the beneficial effects of the present invention are: the preparation method provided by the present invention can simultaneously improve the induced potential and initial magnetic permeability of the ultrafine crystal magnetic core, reduce the magnetic core loss, and the production process is relatively simple and the cost is relatively low, it is easy to realize industrialization, the product produced has excellent soft magnetic properties, the initial magnetic permeability can reach 118,400, under the condition of 50mA excitation current, the induced potential increased by 23.8%, under the condition of 450mA excitation current, the induced potential increased by 4.27%, when the rated current percentage is 1% and 120%, the negative ratio difference is reduced by 0.05%, and the angular difference is reduced by 2.1min and 3min respectively. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 A schematic diagram of the unannealed roller surface of the magnetic core of the present invention is shown;

[0035] Figure 2 A schematic diagram of the unannealed free surface of the magnetic core of the present invention is shown;

[0036] Figure 3 A schematic diagram of the annealing roller surface of the magnetic core of the present invention is shown;

[0037] Figure 4 A schematic diagram of the annealed free surface of the magnetic core of the present invention is shown;

[0038] Figure 5 shows the XRD diffraction pattern of the surface of the strip of the magnetic core of the present invention before annealing;

[0039] Figure 6 The XRD diffraction pattern of the surface of the strip of the magnetic core of the present invention during annealing is shown. DETAILED DESCRIPTION

[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] 1. Materials:

[0042] The ultra-microcrystalline magnetic core is composed of an amorphous and nanocrystalline dual-phase structure, with an average grain size of less than 25nm, and includes iron, copper, niobium, silicon and boron. The molecular formula of the magnetic core is Fe a Cu b Nb c Si d B e .

[0043] Among them, it should be noted that the molecular formula of the ultra-fine crystal magnetic core is: Fe a Cu b Nb c Si d B e ;

[0044] Fe a Cu b Nb c Si d B e a, b, c, d and e are the atomic ratios of the corresponding elements in the alloy, where:

[0045] 0.1≤b≤2;

[0046] 0.5≤c≤5;

[0047] 0.5≤d≤3;

[0048] 6≤e≤12.

[0049] 2. Production of ultra-microcrystalline magnetic core:

[0050] The method for preparing the ultra-microcrystalline magnetic core comprises the following steps:

[0051] S1. The strip is prepared by a single-roller quenching method, and the ejected strip is divided into a free surface and a roller-attached surface;

[0052] Specifically, the steps are:

[0053] S1.1. Prepare a strip with a thickness of 32-36um, a cooling roller speed of 1500-1650r / min, and a strip width of 25mm;

[0054] S1.2. Winding into a toroidal core with an inner diameter of 100 mm, an outer diameter of 123 ± 0.5 mm, a height of 25 mm, and a weight of 600 g;

[0055] S1.3. Use a semi-automatic winding device for manual winding and control the winding weight of the free surface and the roller surface;

[0056] S2. When the vacuum muffle furnace is used for heat treatment, the heating, insulation and cooling process of the wound magnetic core includes the following stages:

[0057] The room temperature was raised to 300°C in 70 minutes;

[0058] Heating from 300℃ to 400℃ takes 120 minutes, and keeping warm for 30 minutes;

[0059] Heating from 400℃ to 480℃ takes 90 minutes, and keeping warm for 90 minutes;

[0060] Heating from 480℃ to 555℃ takes 90 minutes and keeps warm for 60 minutes;

[0061] Finally, cool to below 260℃ and take out of the oven;

[0062] (1) Surface morphology analysis:

[0063] (1.1) Please refer to Figure 1 and Figure 2 The surface morphology of the roller surface and free surface in the unannealed state is described as follows:

[0064] (1.1.1) Roller surface: The surface is relatively rough, with many cooling defects and a darker gloss. This is because during the rapid cooling process, the molten liquid directly contacts the copper roller, and the cooling speed is very fast, which affects the uniformity of the molten liquid layer, resulting in defects such as pits, pores and impurities on the surface. Figure 1 ;

[0065] (1.1.2) Free surface: The surface is relatively smooth, with fewer cooling defects and brighter gloss. This is because the free surface does not directly contact the copper roller during the cooling process, and the cooling speed is relatively slow, retaining the uniform liquid characteristics of the molten liquid layer. Figure 2 ;

[0066] (1.2) Please refer to Figure 3 and Figure 4 The surface morphology of the roller surface and free surface after annealing is described as follows:

[0067] After annealing, the flatness of the surface morphology of both the roller surface and the free surface has been improved, the cooling defects have been reduced, and the roller surface has become relatively smooth. Figure 3 , and the glossiness and uniformity of the free surface are further improved. Figure 4 ;

[0068] (2) Crystal structure analysis:

[0069] The diffraction patterns of the strip samples were analyzed by X-ray diffractometer (model: XRD-7000). By comparing with the PDF card, it was found that the peaks after annealing were all α-Fe phase, and the crystal plane indices of the main diffraction peaks were (110), (200), and (211). The XRD diffraction patterns of the strip surface before and after annealing are shown in Figure 2. Figure 5 and Figure 6 ;

[0070] Analysis of average grain size of free surface and roller surface:

[0071] Free surface: Since the free surface is not subjected to the mechanical action of the cooling roller surface during high-speed cooling and does not directly contact the copper roller, the cooling speed is slow, so the average grain size is relatively large. The average grain size D is calculated to be 14.16nm;

[0072] Roller surface: The roller surface is in direct contact with the copper roller during the cooling process, and the cooling speed is very fast, resulting in a relatively small average grain size. The average grain size D is calculated to be 11.73nm;

[0073] S3. Curing and packaging the heat-treated magnetic core;

[0074] Specifically, the steps are:

[0075] S3.1. Apply epoxy resin AB glue on one side and install it in the ball molding compound protective box;

[0076] S3.2. The dimensions of the protective box are 95mm inner diameter, 130mm outer diameter and 30mm height;

[0077] S4. Winding the solidified and packaged magnetic core. Specifically, the steps are as follows:

[0078] S4.1. Use 1.45 mm and 0.51 mm copper wires in parallel to surround the core, with the wires evenly spaced.

[0079] S4.2. The number of turns of 0.51mm copper wire is one less than that of 1.45mm.

[0080] Comparative Example

[0081] In this comparative example, the overall preparation process of the ultra-microcrystalline magnetic core remains unchanged, and the winding weights of the free surface and the roller surface are controlled as follows in step S1.3:

[0082] Free noodles: 600g;

[0083] Roller surface: 0g;

[0084] An ultra-microcrystalline magnetic core with sample number 1 was prepared by the above process.

[0085] Example 1

[0086] In this embodiment, the overall preparation process of the ultra-microcrystalline magnetic core remains unchanged, and the winding weight of the free surface and the roller surface is controlled as follows in step S1.3:

[0087] Free noodles: 450g;

[0088] Roller surface: 150g;

[0089] The ultra-microcrystalline magnetic core with sample number 2 was prepared by the above process.

[0090] Example 2

[0091] In this embodiment, the overall preparation process of the ultra-microcrystalline magnetic core remains unchanged, and the winding weight of the free surface and the roller surface is controlled as follows in step S1.3:

[0092] Free noodles: 300g;

[0093] Roller surface: 300g;

[0094] The ultra-microcrystalline magnetic core with sample number three was prepared by the above process.

[0095] Example 3

[0096] In this embodiment, the overall preparation process of the ultra-microcrystalline magnetic core remains unchanged, and the winding weight of the free surface and the roller surface is controlled as follows in step S1.3:

[0097] Free noodles: 150g;

[0098] Roller surface: 450g;

[0099] The ultra-microcrystalline magnetic core with sample number 4 was prepared by the above process.

[0100] Example 4

[0101] In this embodiment, the overall preparation process of the ultra-microcrystalline magnetic core remains unchanged, and the winding weight of the free surface and the roller surface is controlled as follows in step S1.3:

[0102] Free noodles: 0g;

[0103] Roller surface: 600g;

[0104] The ultra-microcrystalline magnetic core with sample number five was prepared by the above process.

[0105] 3. Performance test:

[0106] The comparison table of the winding weight of the free surface and the roller surface of the ultra-microcrystalline magnetic core in the above sample No. 1 to No. 5 is shown in Table 1:

[0107] Table 1 Comparison of free surface and roller surface winding weight

[0108] Example No. Free surface winding weight (g) Roller surface winding weight (g) Comparative Example 600 0 Example 1 450 150 Example 2 300 300 Example 3 150 450 Example 4 0 600

[0109] The performance tests were conducted on the ultra-microcrystalline magnetic cores in product numbers 1 to 5:

[0110] (1) The loss of the ultra-microcrystalline core was measured using an automatic AC magnetic properties test system (model MATS-2010SA). The test was carried out under sinusoidal alternating current conditions with a test frequency of 50 Hz:

[0111] (1.1) When the magnetic induction intensity is 0.8T:

[0112] The loss values ​​(W / kg) of sample scheme numbers 1 to 5 are:

[0113] Sample solution number 1: 0.459×10 -3 ;

[0114] Sample solution number 2: 0.417×10 -3 ;

[0115] Sample solution number three: 0.3080×10 -3 ;

[0116] Sample solution number 4: 0.338×10 -3 ;

[0117] Sample plan number five: 0.437×10 -3 .

[0118] (1.2) When the magnetic induction intensity is 0.1T:

[0119] The loss values ​​(W / kg) of sample scheme numbers 1 to 5 are:

[0120] Sample plan number 1: 20.4×10 -3 ;

[0121] Sample plan number 2: 19.9×10 -3 ;

[0122] Sample plan number three: 18.5×10 -3 ;

[0123] Sample plan number 4: 018.9×10 -3 ;

[0124] Sample plan number five: 21.0×10 -3 ;

[0125] (2) Use a high-precision LCR meter (model TH-2826A) to measure the inductance AL of the magnetic ring, and convert the inductance to solve the magnetic permeability, see formula (1):

[0126]

[0127] Where AL is the inductance, l e is the effective magnetic path length, μ0 is the vacuum magnetic permeability, N is the number of winding turns, A e is the effective magnetic circuit cross-sectional area;

[0128] The test voltage is 0.3V, the internal resistance is 30Ω, and the measurement frequency is 1KHz;

[0129] Relative magnetic permeability (u e) are:

[0130] Sample solution number 1: 9.74×10 4 ;

[0131] Sample solution number 2: 10.97×10 4 ;

[0132] Sample plan number three: 11.84×10 4 ;

[0133] Sample solution number 4: 11.15×10 4 ;

[0134] Sample plan number five: 10.24×10 4 ;

[0135] (3) Use an iron core magnetic property measuring instrument (model HD1) to measure the induced potential value of the magnetic core sample;

[0136] (3.1) When the excitation current is 50mA:

[0137] The induced potentials (mV) of sample scheme numbers 1 to 5 are:

[0138] Sample plan number 1: 2.1;

[0139] Sample plan number two: 2.5;

[0140] Sample plan number three: 2.6;

[0141] Sample plan number four: 2.4;

[0142] Sample plan number five: 2.1;

[0143] The ultra-microcrystalline core induced potential of sample solution No. 3 is the highest, reaching 2.6mV, which is 23.8% higher than that of sample solution No. 1 (comparative example);

[0144] (3.2) When the excitation current is 450mA:

[0145] The induced potentials (mV) of sample scheme numbers 1 to 5 are:

[0146] Sample plan number 1: 52.5;

[0147] Sample plan number 2: 55.0;

[0148] Sample plan number three: 55.1;

[0149] Sample plan number four: 53.1;

[0150] Sample plan number five: 50.7;

[0151] The induced potential of sample solution No. 3 is still the highest, reaching 55.1 mV, which is 4.27% higher than that of sample solution No. 1 (comparative example);

[0152] (4) Use a mutual inductor error calibrator (model SZCP-2) to measure the ratio error and angle error of the sample;

[0153] (4.1) When the percentage of rated current is 1%, the ratio difference (%) and angle difference (%) of sample scheme numbers 1 to 5 are:

[0154] The ratio difference of sample scheme number 1: -0.13;

[0155] The ratio difference of sample scheme number 2: -0.12;

[0156] The ratio difference of sample scheme number three: -0.07;

[0157] The ratio difference of sample scheme number four: -0.10;

[0158] The ratio difference of sample scheme number five: -0.12;

[0159] Therefore, when the percentage of rated current is 1%, the sample solution number 3 has the lowest ratio difference, which is -0.07%;

[0160] The angle difference of sample plan number 1: 16.80;

[0161] The angle difference of sample plan number 2: 16.30;

[0162] The angular difference of sample plan number three: 14.70;

[0163] The angle difference of sample plan number four: 15.40;

[0164] The angular difference of sample plan number five: 16.50;

[0165] Therefore, when the percentage of rated current is 1%, the angle difference of sample solution number 3 is also the lowest, which is 14.70%;

[0166] (4.2) When the percentage of rated current is 120%, the ratio difference (%) and angle difference (%) of sample scheme numbers 1 to 5 are:

[0167] The ratio difference of sample scheme number 1: -0.05;

[0168] The ratio difference of sample scheme number 2: -0.02;

[0169] Ratio difference of sample plan number three: 0.00;

[0170] The ratio difference of sample scheme number four: -0.06;

[0171] The ratio difference of sample scheme number five: -0.08;

[0172] Therefore, when the percentage of rated current is 120%, the ratio difference of sample solution number 3 is still the best, which is 0.00%.

[0173] The angle difference of sample plan number 1: 6.80;

[0174] The angle difference of sample plan number 2: 4.30;

[0175] Angular difference of sample plan number three: 3.0;

[0176] The angular difference of sample plan number four: 9.8;

[0177] The angular difference of sample plan number five: 10.1;

[0178] Therefore, when the percentage of rated current is 120%, the angle difference of sample solution number 3 is the lowest, which is 3.09%;

[0179] In summary, by testing and analyzing the various properties of the ultra-microcrystalline magnetic core under different experimental schemes, it can be found that in the comparative examples and embodiments 1 to 5, the sample scheme No. 3 (free surface 300g, roller surface 300g) prepared by embodiment 2 shows better performance in ultra-microcrystalline magnetic core loss, initial magnetic permeability, induced potential and error control. Therefore, in the preparation process of the ultra-microcrystalline magnetic core, embodiment 2 is the best embodiment. Therefore, the preparation method provided by the present invention can simultaneously improve the ultra-microcrystalline magnetic core. The induced potential and initial magnetic permeability can reduce the core loss, and the production process is relatively simple and the cost is relatively low, which is easy to realize industrialization. The products have excellent soft magnetic properties, and the initial magnetic permeability can reach 118,400. Under the condition of 50mA excitation current, the induced potential increases by 23.8%, and under the condition of 450mA excitation current, the induced potential increases by 4.27%. When the rated current percentage is 1% and 120%, the negative ratio difference is reduced by 0.05%, and the angular difference is reduced by 2.1min and 3min respectively.

[0180] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An ultra-microcrystalline magnetic core, the magnetic core is composed of an amorphous and nanocrystalline dual-phase structure, the average grain size is less than 25nm, characterized in that: The magnetic core comprises iron, copper, niobium, silicon and boron. The molecular formula of the magnetic core is Fe a Cu b Nb c Si d B e .

2. The ultra-microcrystalline magnetic core according to claim 1, characterized in that: The magnetic core molecular formula is Fe a Cu b Nb c Si d B e Where a, b, c, d and e are the atomic ratios of the corresponding elements in the alloy, where: 0.1≤b≤2; 0.5≤c≤5; 0.5≤d≤3; 6≤e≤12。 3. A method for preparing an ultra-microcrystalline magnetic core, according to any one of claims 1-2, characterized in that: The following steps are involved: S1. The strip is prepared by a single-roller quenching method, and the ejected strip is divided into a free surface and a roller-attached surface; S2. Heat treatment of the wound magnetic core is performed using a vacuum muffle furnace; S3. Curing and packaging the heat-treated magnetic core; S4. Wind the solidified and packaged magnetic core.

4. The method for preparing the ultrafine crystal magnetic core according to claim 3, characterized in that: The strip preparation in step S1 comprises the following steps: S1.

1. Prepare a strip with a thickness of 32-36um, a cooling roller speed of 1500-1650r / min, and a strip width of 25mm; S1.

2. Winding into a toroidal core with an inner diameter of 100 mm, an outer diameter of 123 ± 0.5 mm, a height of 25 mm, and a weight of 600 g; S1.

3. Use a semi-automatic winding device for manual winding and control the winding weight of the free side and the roller side.

5. The method for preparing the ultra-microcrystalline magnetic core according to claim 3, characterized in that: When the vacuum muffle furnace is used for heat treatment in step S2, the heating, insulation and cooling process of the wound magnetic core includes the following stages: The room temperature was raised to 300°C in 70 minutes; Heating from 300℃ to 400℃ takes 120 minutes, and keeping warm for 30 minutes; Heating from 400℃ to 480℃ takes 90 minutes, and keeping warm for 90 minutes; Heating from 480℃ to 555℃ takes 90 minutes and keeps warm for 60 minutes; Finally, it is cooled to below 260°C and taken out of the oven.

6. The method for preparing the ultra-microcrystalline magnetic core according to claim 3, characterized in that: The curing and packaging process of step S3 is as follows: S3.

1. Apply epoxy resin AB glue on one side and install it in the ball molding compound protective box; S3.

2. The dimensions of the protective box are inner diameter 95mm, outer diameter 130mm and height 30mm.

7. The method for preparing the ultra-microcrystalline magnetic core according to claim 3, characterized in that: The winding process of step S4 is as follows: S4.

1. Use 1.45 mm and 0.51 mm copper wires in parallel to surround the core, with the wires evenly spaced. S4.

2. The number of turns of 0.51mm copper wire is one less than that of 1.45mm.

Citation Information

Cited By

  • Current transformer magnetic core heat treatment method for optimizing magnetic domain structure

    CN120432297A

  • Wide-range current transformer

    CN121416290A