Negative plate, preparation method thereof and battery monomer
By adopting a combined structure of lithium metal layer, internal suppression layer and external suppression layer in lithium metal batteries, safety hazards and performance bottlenecks caused by dendrites are solved, and the cycle life and safety of the battery are significantly improved.
Patent Information
- Application Number
- CN202411040391.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-29
AI Technical Summary
Dental growth is caused by uneven metal deposition in lithium metal batteries, which poses safety risks and hinders the development of high-energy-density batteries.
The negative electrode sheet design is adopted including a lithium metal layer, an internal suppression layer and an external suppression layer. The internal suppression layer is composed of a polymer large anion lithium salt and a first polymer. The external suppression layer is composed of a cuprous compound, and the excess is captured through these hierarchical structures. The uniform conduction of electrons and lithium ions is controlled to inhibit dendrites.
It effectively improves the cycle life and safety of the battery, reduces the formation of dendrites, and improves the overall performance of the battery.
Smart Images

Figure CN119050271A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of secondary batteries, and in particular to a negative electrode sheet and a preparation method thereof, and a battery cell. Background Art
[0002] Lithium-ion batteries have dominated the energy storage market for many years due to their unique intercalation / deintercalation mechanism. However, despite significant optimization, there is still a large gap between the energy density of "rocking chair" type lithium-ion batteries and the requirements of emerging industries. For the ultimate choice of the new generation of high energy density systems, metallic lithium (Li) is known for its high capacity (10 times higher than graphite anode), the lowest redox potential (-3.04V) and light mass density (0.534g cm-3). At the same time, the chemical process of lithium-based batteries involves repeated lithium plating and delithiation processes. Due to the defective substrate and "frameless" nature, lithium metal anodes inevitably induce dendrite deposition and uncontrollable volume changes, which hinders their further development. Therefore, high energy density lithium anodes with well-guided lithium deposition behavior and optimized electrochemical performance are very important. The advantages of using metallic lithium as anode have been proven in non-rechargeable lithium batteries, and they are quickly applied to power sources such as watches, computers and implantable medical devices due to their high capacity and variable discharge rate. At the same time, many inorganic materials have been found to react reversibly with alkali metals, which are called intercalation compounds. The discovery of these materials is crucial to the development of high-energy rechargeable lithium battery systems. Some people have proposed using TiS2 as the positive electrode, metallic lithium as the negative electrode, dioxolane (DOL) as the electrolyte solvent, and lithium perchlorate (LiClO4) as the electrolyte solute to construct a rechargeable lithium metal battery. Although this work has received widespread attention, it was soon discovered that due to the contact problem between the metallic lithium negative electrode and the liquid electrolyte, the uneven metal deposition process in each charge and discharge cycle leads to the growth of metallic lithium dendrites, which can cause the battery to explode. In order to solve the various safety problems existing in lithium metal batteries, researchers have adopted many different methods, including various modifications of electrolyte materials and the use of embedded negative electrode materials to replace the metallic lithium negative electrode, but the effect is still not ideal. Summary of the invention
[0003] The present application provides a negative electrode sheet and a preparation method thereof, and a battery cell, so as to improve the problem that the negative electrode sheet of the battery is prone to dendrite generation.
[0004] In a first aspect, the present application provides a negative electrode sheet, which includes a lithium metal layer, an internal inhibition layer and an external inhibition layer, wherein the lithium metal layer is arranged between the internal inhibition layer and the external inhibition layer; the internal inhibition layer includes a first organic layer, and the components of the first organic layer include a polymer large anion lithium salt and a first polymer; the components of the external inhibition layer include a cuprous compound.
[0005] As an optional embodiment, the internal inhibition layer also includes an inorganic layer and a second organic layer, the first organic layer, the inorganic layer and the second organic layer are stacked in sequence, and the first organic layer is arranged between the lithium metal layer and the inorganic layer, the components of the inorganic layer include an oxide ceramic electrolyte, and the components of the second organic layer include a second polymer and a lithium salt.
[0006] As an optional embodiment, the polymer macroanion lithium salt comprises
[0007]
[0008] At least one of;
[0009] As an optional embodiment, the first polymer includes polyvinylidene fluoride-hexafluoropropylene; and / or
[0010] The mass ratio of the polymer macroanion lithium salt to the first polymer is (2-10):1.
[0011] As an optional embodiment, the cuprous compound includes at least one of cuprous oxide and cuprous nitride.
[0012] As an optional embodiment, the oxide ceramic electrolyte includes at least one of lithium aluminum titanium phosphate, lithium lanthanum zirconate and tantalum-doped lithium lanthanum zirconate.
[0013] As an optional embodiment, the second polymer includes at least one of polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, polycaprolactone, polypropylene polycarbonate and polyimide; and / or
[0014] The lithium salt comprises at least one of lithium perchlorate, lithium bis(trifluoromethanesulfonate imide), lithium bis(fluorosulfonamide), lithium difluorooxalatoborate, lithium hexafluorophosphate, lithium tetrafluoroborate and lithium hexafluoroarsenate; and / or
[0015] The mass ratio of the second polymer to the lithium salt is (3-12):1.
[0016] As an optional embodiment, the thickness of the lithium metal layer is 15 μm to 65 μm; and / or
[0017] The thickness of the first organic layer is 15 μm to 25 μm; and / or
[0018] The thickness of the inorganic layer is 25 μm to 60 μm; and / or
[0019] The thickness of the second organic layer is 15 μm to 35 μm; and / or
[0020] The thickness of the external inhibition layer is 10 μm to 20 μm.
[0021] In a second aspect, the present application provides a method for preparing a negative electrode sheet, wherein the negative electrode sheet is the negative electrode sheet provided in the first aspect; the method comprises:
[0022] Obtaining a lithium metal layer;
[0023] Prepare an external inhibition layer on one surface of the lithium metal layer to obtain an intermediate product;
[0024] An internal inhibition layer is formed on the other surface of the lithium metal layer of the intermediate product to obtain a negative electrode sheet.
[0025] In a third aspect, the present application provides a battery cell, wherein the battery cell comprises the negative electrode sheet provided in the first aspect.
[0026] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0027] The negative electrode sheet provided in the embodiment of the present application has an external inhibition layer composed of a cuprous compound arranged on one side of the lithium metal layer, which can capture excess electrons, prevent excessive polarization due to excessive electron accumulation, and inhibit the formation of lithium dendrites. At the same time, an internal inhibition layer composed of a polymer large anion lithium salt is arranged on the other side of the lithium metal layer, which effectively controls the uniform conduction of lithium ions and inhibits the formation of lithium dendrites, thereby improving the battery cycle life and battery safety. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0029] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0030] Figure 1 A schematic diagram of the structure of the negative electrode sheet provided in an embodiment of the present application;
[0031] Figure 2 A schematic diagram of a process for a method provided in an embodiment of the present application;
[0032] Figure 3 A graph showing the cycle test results provided in Example 1 of the present application;
[0033] Figure 4A graph showing the results of a cycle test provided in Example 2 of the present application;
[0034] Figure 5 A graph showing the cycle test results provided in Example 3 of the present application;
[0035] Figure 6 A graph showing the cycle test results provided in Example 4 of the present application;
[0036] Figure 7 A graph showing the results of a cycle test provided for Comparative Example 1 of the present application;
[0037] Figure 8 A graph showing the results of a cycle test provided for Comparative Example 2 of this application;
[0038] Fig. 9 This is a graph of the cycle test results provided for Comparative Example 3 of the present application.
[0039] Reference numerals: 1 - lithium metal layer, 2 - internal inhibition layer, 21 - first organic layer, 22 - inorganic layer, 23 - second organic layer, 3 - external inhibition layer. DETAILED DESCRIPTION
[0040] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0041] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0042] Figure 1 A schematic diagram of the structure of the negative electrode sheet provided in the embodiment of the present application is shown in FIG. Figure 1 As shown, an embodiment of the present application provides a negative electrode sheet, which includes a lithium metal layer, an internal inhibition layer and an external inhibition layer, wherein the lithium metal layer is arranged between the internal inhibition layer and the external inhibition layer; the internal inhibition layer includes a first organic layer, and the components of the first organic layer include a polymer large anion lithium salt and a first polymer; the components of the external inhibition layer include a cuprous compound.
[0043] The negative electrode sheet has an external inhibition layer composed of a cuprous compound on one side of the lithium metal layer, which can capture excess electrons, prevent excessive polarization due to excessive electron accumulation, and inhibit the formation of lithium dendrites. At the same time, an internal inhibition layer composed of a polymer large anion lithium salt is arranged on the other side of the lithium metal layer, which effectively controls the uniform conduction of lithium ions and inhibits the formation of lithium dendrites, thereby improving the battery cycle life and battery safety.
[0044] In some embodiments, the polymeric macroanion lithium salt comprises
[0045]
[0046] At least one of the following: the first polymer includes polyvinylidene fluoride-hexafluoropropylene. Furthermore, the mass ratio of the polymer macroanion lithium salt to the first polymer is (2-10):1.
[0047] In some embodiments, the cuprous compound includes at least one of cuprous oxide (Cu2O) and cuprous nitride (Cu3N). Cuprous oxide (Cu2O) or cuprous nitride (Cu3N) serves as an external inhibition layer to capture excess electrons, prevent excessive polarization due to excessive electron accumulation, inhibit lithium dendrite formation, and thereby improve battery cycle life and battery safety.
[0048] In some embodiments, the internal inhibition layer also includes an inorganic layer and a second organic layer, the first organic layer, the inorganic layer and the second organic layer are stacked in sequence, and the first organic layer is arranged between the lithium metal layer and the inorganic layer, the components of the inorganic layer include an oxide ceramic electrolyte, and the components of the second organic layer include a second polymer and a lithium salt.
[0049] The provision of an inorganic layer composed of an oxide ceramic electrolyte and a second organic layer composed of a second polymer and a lithium salt can improve the lithium ion conduction efficiency.
[0050] In some embodiments, the oxide ceramic electrolyte includes at least one of lithium aluminum titanium phosphate (LATP), lithium lanthanum zirconate (LLZO), and tantalum-doped lithium lanthanum zirconate (LLZTO).
[0051] In some embodiments, the second polymer includes at least one of polyethylene oxide (PEO), polyacrylonitrile (PAN), polyvinylidene fluoride (PVDF), polycaprolactone (PCL), polypropylene polycarbonate (PPC), and polyimide (PI); the lithium salt includes at least one of lithium perchlorate (LiClO4), lithium bis(trifluoromethanesulfonimide) (LiTFSI), lithium bis(fluorosulfonimide) (LiFSI), lithium difluorooxalatoborate (LiDFOB), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), and lithium hexafluoroarsenate (LiAsPF6); the mass ratio of the second polymer to the lithium salt is (3 to 12):1.
[0052] Exemplarily, the mass ratio of the second polymer to the lithium salt may be 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1 or 12:1, etc., and may also be any value within the range of (3-12):1.
[0053] In some embodiments, the thickness of the lithium metal layer is 15 μm to 65 μm; the thickness of the first organic layer is 15 μm to 25 μm; the thickness of the inorganic layer is 25 μm to 60 μm; the thickness of the second organic layer is 15 μm to 35 μm; and the thickness of the external inhibition layer is 10 μm to 20 μm.
[0054] Figure 2 A flow chart of the method provided in the embodiment of the present application is as follows: Figure 2 As shown, based on a general inventive concept, an embodiment of the present application further provides a method for preparing a negative electrode sheet, wherein the negative electrode sheet is the negative electrode sheet provided above.
[0055] The method is used for preparing the above-mentioned negative electrode sheet. The specific content of the negative electrode sheet can refer to the above-mentioned embodiment. Since the method adopts part or all of the technical solutions of the above-mentioned embodiment, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiment, which will not be repeated here one by one.
[0056] In some embodiments, the method comprises:
[0057] S1. Obtaining a lithium metal layer;
[0058] S2. Preparing an external inhibition layer on a surface of the lithium metal layer to obtain an intermediate;
[0059] Specifically, in this embodiment, cuprous oxide (Cu2O) and / or cuprous nitride (Cu3N) is sprayed on one side of the lithium metal layer by spraying to obtain an intermediate product.
[0060] S3. Prepare an internal inhibition layer on the other surface of the lithium metal layer of the intermediate product to obtain a negative electrode sheet.
[0061] Specifically, in this embodiment, first, a polymer large anion lithium salt and a first polymer polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) are mixed in a certain proportion and then put into a hot press for internal kneading. After internal kneading, a uniform slurry is formed. The slurry is hot pressed on the other surface of the lithium metal layer to form a first organic layer; an oxide ceramic electrolyte is sprayed on the first organic layer by spraying to form an inorganic layer; an organic coating is hot pressed on the inorganic layer again, and the organic coating is formed into a uniform slurry by internal kneading with a second polymer and a lithium salt, and is sprayed on the inorganic layer by spraying to form a second organic layer, thereby obtaining a negative electrode sheet.
[0062] Based on a general inventive concept, an embodiment of the present application further provides a battery cell, wherein the battery cell includes the negative electrode sheet provided above.
[0063] The battery cell is implemented based on the above-mentioned negative electrode sheet. The specific content of the negative electrode sheet can refer to the above-mentioned embodiment. Since the battery cell adopts part or all of the technical solutions of the above-mentioned embodiments, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be repeated here one by one.
[0064] In some embodiments, the battery cell further includes a positive electrode sheet and a solid electrolyte layer, the solid electrolyte layer is disposed between the positive electrode sheet and the negative electrode sheet, and the internal inhibition layer of the negative electrode sheet is disposed in contact with the solid electrolyte layer.
[0065] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0066] Example 1
[0067] A battery cell, the preparation process is as follows:
[0068] The ratio of ternary material (NCM811), adhesive polytetrafluoroethylene emulsion (PTFE), and conductive agent is 95:3:2, mixed evenly, and then coated on the current collector aluminum foil to obtain a positive electrode sheet;
[0069] Cuprous nitride (Cu3N) is sprayed on one side of the lithium metal layer; PVDF-HFP and a large anion lithium salt are dissolved in N,N-dimethylformamide (DMF), mixed evenly, and then sprayed on the other side of the lithium metal layer to obtain a first organic layer; a solid electrolyte is dissolved in N,N-dimethylformamide (DMF), mixed evenly, and then sprayed on the first organic layer to form an inorganic layer; PEO-PCL-LFSI is dissolved in dimethyl carbonate (DMC) at a mass ratio of 4:4:2, and then sprayed on the inorganic layer to form a second organic layer to obtain a negative electrode sheet;
[0070] The positive and negative electrode sheets are assembled to obtain a battery cell.
[0071] Example 2
[0072] A battery cell, the preparation process is as follows:
[0073] The ratio of ternary material (NCM811), adhesive polytetrafluoroethylene emulsion (PTFE), and conductive agent is 95:3:2, mixed evenly, and then coated on the current collector aluminum foil to obtain a positive electrode sheet;
[0074] Spraying cuprous oxide (Cu2O) on one side of the lithium metal layer; dissolving PVDF-HFP and a large anion lithium salt in N,N-dimethylformamide (DMF), mixing them evenly and spraying them on the other side of the lithium metal layer to obtain a first organic layer; dissolving a solid electrolyte in N,N-dimethylformamide (DMF), mixing them evenly and spraying them on the first organic layer to form an inorganic layer; dissolving PEO-PCL-LFSI in dimethyl carbonate (DMC) at a mass ratio of 4:4:2, and then spraying them on the inorganic layer to form a second organic layer to obtain a negative electrode sheet;
[0075] The positive and negative electrode sheets are assembled to obtain a battery cell.
[0076] Example 3
[0077] A battery cell, the preparation process is as follows:
[0078] The ratio of ternary material (NCM811), adhesive polytetrafluoroethylene emulsion (PTFE), and conductive agent is 95:3:2, mixed evenly, and then coated on the current collector aluminum foil to obtain a positive electrode sheet;
[0079] Cuprous oxide (Cu2O) is sprayed on one side of the lithium metal layer; PVDF-HFP and a large anion lithium salt are dissolved in N,N-dimethylformamide (DMF), mixed evenly, and then sprayed on the other side of the lithium metal layer to obtain a first organic layer; a solid electrolyte is dissolved in N,N-dimethylformamide (DMF), mixed evenly, and then sprayed on the first organic layer to form an inorganic layer; PVDF-PPC-LFSI is dissolved in dimethyl carbonate (DMC) at a mass ratio of 2:6:2, and then sprayed on the inorganic layer to form a second organic layer to obtain a negative electrode sheet;
[0080] The positive and negative electrode sheets are assembled to obtain a battery cell.
[0081] Example 4
[0082] A battery cell, the preparation process is as follows:
[0083] The ratio of ternary material (NCM811), adhesive polytetrafluoroethylene emulsion (PTFE), and conductive agent is 95:3:2, mixed evenly, and then coated on the current collector aluminum foil to obtain a positive electrode sheet;
[0084] Cuprous nitride (Cu3N) is sprayed on one side of the lithium metal layer; PVDF-HFP and a large anion lithium salt are dissolved in N,N-dimethylformamide (DMF), mixed evenly, and then sprayed on the other side of the lithium metal layer to obtain a first organic layer; a solid electrolyte is dissolved in N,N-dimethylformamide (DMF), mixed evenly, and then sprayed on the first organic layer to form an inorganic layer; PVDF-PPC-LFSI is dissolved in dimethyl carbonate (DMC) at a mass ratio of 2:6:2, and then sprayed on the inorganic layer to form a second organic layer to obtain a negative electrode sheet;
[0085] The positive and negative electrode sheets are assembled to obtain a battery cell.
[0086] Comparative Example 1
[0087] A battery cell, the preparation process is as follows:
[0088] The ratio of ternary material (NCM811), adhesive polytetrafluoroethylene emulsion (PTFE), and conductive agent is 95:3:2, mixed evenly, and then coated on the current collector aluminum foil to obtain a positive electrode sheet;
[0089] A negative electrode sheet is obtained by spraying cuprous nitride (Cu3N) on one side of the lithium metal layer;
[0090] The positive and negative electrode sheets are assembled to obtain a battery cell.
[0091] Comparative Example 2
[0092] A battery cell, the preparation process is as follows:
[0093] The ratio of ternary material (NCM811), adhesive polytetrafluoroethylene emulsion (PTFE), and conductive agent is 95:3:2, mixed evenly, and then coated on the current collector aluminum foil to obtain a positive electrode sheet;
[0094] PVDF-HFP and a large anion lithium salt are dissolved in N,N-dimethylformamide (DMF), mixed evenly, and then sprayed on one side of the lithium metal layer to obtain a first organic layer; a solid electrolyte is dissolved in N,N-dimethylformamide (DMF), mixed evenly, and then sprayed on the first organic layer to form an inorganic layer; PEO-PCL-LFSI is dissolved in dimethyl carbonate (DMC) at a mass ratio of 4:4:2, and then sprayed on the inorganic layer to form a second organic layer to obtain a negative electrode sheet;
[0095] The positive and negative electrode sheets are assembled to obtain a battery cell.
[0096] Comparative Example 3
[0097] A battery cell, the preparation process is as follows:
[0098] The ratio of ternary material (NCM811), adhesive polytetrafluoroethylene emulsion (PTFE), and conductive agent is 95:3:2, mixed evenly, and then coated on the current collector aluminum foil to obtain a positive electrode sheet;
[0099] The metal lithium layer is used as the negative electrode;
[0100] The positive and negative electrode sheets are assembled to obtain a battery cell.
[0101] The battery cells provided in each embodiment and comparative example were subjected to 100 cycles of cycling test at a cycle rate of 1C, and the lithium dendrites were observed. The results are as follows: Figures 3 to 9 And the following table shows:
[0102] Capacity retention rate Lithium dendrite situation Example 1 99.58% none Example 2 100.06% none Example 3 99.55% none Example 4 99.30% none Comparative Example 1 59.93% Presence of lithium dendrites Comparative Example 2 65.09% Presence of lithium dendrites Comparative Example 3 0.30% There are a lot of lithium dendrites
[0103] It can be seen from the accompanying drawings and the above table that the negative electrode sheet provided in the embodiment of the present application can effectively improve the dendrite situation of the battery cell.
[0104] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0105] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b and c can be single or multiple.
[0106] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A negative electrode sheet, characterized in that: The negative electrode sheet includes a lithium metal layer, an internal inhibition layer and an external inhibition layer, wherein the lithium metal layer is arranged between the internal inhibition layer and the external inhibition layer; the internal inhibition layer includes a first organic layer, the components of which include a polymer large anion lithium salt and a first polymer; and the components of the external inhibition layer include a cuprous compound.
2. The negative electrode sheet according to claim 1, characterized in that: The internal inhibition layer also includes an inorganic layer and a second organic layer, the first organic layer, the inorganic layer and the second organic layer are stacked in sequence, and the first organic layer is arranged between the lithium metal layer and the inorganic layer, the components of the inorganic layer include an oxide ceramic electrolyte, and the components of the second organic layer include a second polymer and a lithium salt.
3. The negative electrode sheet according to claim 1 or 2, characterized in that: The polymer macroanion lithium salt comprises: At least one of .
4. The negative electrode sheet according to claim 3, characterized in that: The first polymer comprises polyvinylidene fluoride-hexafluoropropylene; and / or The mass ratio of the polymer macroanion lithium salt to the first polymer is (2-10):
1.
5. The negative electrode sheet according to claim 1 or 2, characterized in that: The cuprous compound includes at least one of cuprous oxide and cuprous nitride.
6. The negative electrode sheet according to claim 2, characterized in that: The oxide ceramic electrolyte includes at least one of lithium aluminum titanium phosphate, lithium lanthanum zirconate, and tantalum-doped lithium lanthanum zirconate.
7. The negative electrode sheet according to claim 2, characterized in that: The second polymer comprises at least one of polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, polycaprolactone, polypropylene polycarbonate and polyimide; and / or The lithium salt comprises at least one of lithium perchlorate, lithium bis(trifluoromethanesulfonate imide), lithium bis(fluorosulfonamide), lithium difluorooxalatoborate, lithium hexafluorophosphate, lithium tetrafluoroborate and lithium hexafluoroarsenate; and / or The mass ratio of the second polymer to the lithium salt is (3-12):
1.
8. The negative electrode sheet according to claim 2, characterized in that: The thickness of the lithium metal layer is 15 μm to 65 μm; and / or The thickness of the first organic layer is 15 μm to 25 μm; and / or The thickness of the inorganic layer is 25 μm to 60 μm; and / or The thickness of the second organic layer is 15 μm to 35 μm; and / or The thickness of the external inhibition layer is 10 μm to 20 μm.
9. A method for preparing a negative electrode sheet, characterized in that: The negative electrode sheet is the negative electrode sheet according to any one of claims 1 to 8; the method comprises: Obtaining a lithium metal layer; Prepare an external inhibition layer on one surface of the lithium metal layer to obtain an intermediate product; An internal inhibition layer is formed on the other surface of the lithium metal layer of the intermediate product to obtain a negative electrode sheet.
10. A battery cell, characterized in that: The battery cell comprises the negative electrode sheet according to any one of claims 1 to 8.