Lithium manganese iron phosphate positive plate and preparation method thereof

CN119050285APending Publication Date: 2024-11-29SHANGHAI RUIPU ENERGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411166022.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Lithium manganese iron phosphate (LMFP) in lithium-ion batteries has poor electronic conductivity and ionic conductivity, resulting in insufficient dynamic performance. Commonly used improvement methods such as compounding and lithium supplementation increase cost and safety risks. , Nanoization treatment has problems with process difficulty and stability.

Method used

By increasing the microwave irradiation power in a gradient, nano iron phosphate material is grown in situ on nickel foam, combining microwave irradiation hydrothermal acid etching and carbon coating to build a good conductive network and improve the lithium ion transmission path and material stability. sex.

Benefits of technology

The preparation of nano-number lithium manganese iron phosphate cathode sheets without binder has been achieved, which improves electrochemical performance and stability, overcomes the problems of poor kinetic performance and process difficulties, reduces the agglomeration of materials and metal ions dissolution, and improves the Battery magnification and cycling performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050285A_ABST
    Figure CN119050285A_ABST
Patent Text Reader

Abstract

The preparation method comprises the following steps: uniformly mixing an iron source, a manganese source, a phosphorus source, a lithium source and a doping element source, then adding foamed nickel, and increasing microwave irradiation power in a gradient manner so as to grow a nano lithium manganese iron phosphate material on the foamed nickel; under microwave irradiation, carrying out acid etching on the nanometer lithium iron manganese phosphate material on the foamed nickel to obtain an etched lithium iron manganese phosphate positive plate; and transferring the etched lithium manganese iron phosphate positive plate into an organic carbon source, and carrying out carbon coating under microwave irradiation to obtain the carbon-coated lithium manganese iron phosphate positive plate. According to the preparation method, the microwave irradiation power is increased in a gradient mode, the nanometer lithium iron manganese phosphate material grows on the foamed nickel in situ, a binding agent is not needed, the electron transmission path is greatly improved, agglomeration of the nanometer lithium iron manganese phosphate material is greatly reduced through the self-supporting foamed nickel, shuttling of lithium ions is facilitated, and a good conductive network is constructed. And then carrying out microwave irradiation hydrothermal acid etching and carbon coating to obtain the lithium manganese iron phosphate positive plate with excellent performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion battery materials, and in particular to a lithium iron manganese phosphate positive electrode sheet and a preparation method thereof. Background Art

[0002] Lithium manganese iron phosphate (LMFP) is generally considered to be an upgraded version of lithium iron phosphate (LFP) in the lithium-ion battery industry because of its higher self-discharge platform (~3.58V) and its gram capacity is comparable to that of lithium iron phosphate (LFP). However, due to its poor electronic and ionic conductivity, LMFP often fails to exert its actual capacity in practical applications.

[0003] At present, most battery manufacturers compound LMFP with nickel cobalt manganese oxide (NCM) to increase the dynamic performance of LMFP to a certain extent. However, due to the introduction of NCM, the cost of the entire system increases by 20% to 30%, and with the increase of NCM, the safety risk of the battery cell inevitably increases.

[0004] Some battery manufacturers also improve the kinetic performance of the system by adding lithium supplement Li5MO4 to the LMFP system, where M includes at least one of Fe, Ni, Mn, Ru, Cr, Cu, Nb, Al or Mo. The lithium supplement is generally an inorganic salt with a high oxygen content. Under high voltage, a large amount of oxygen O2 will be released, resulting in difficult-to-solve interface problems during the battery formation process. In addition, LMFP is a high-voltage system. If the lithium supplement cannot be consumed during the formation process, it will greatly affect the subsequent long-term performance of the battery cell.

[0005] In addition, some material manufacturers have further improved the electrochemical performance of LMFP through nano-sizing, ion doping and carbon coating. Among them, nano-sizing can reduce the solid-phase transmission path of lithium ions and greatly improve the intrinsic kinetics of the material. However, since the particles reach the nanometer level, the increase in specific surface area will bring about extremely high difficulty in subsequent slurry processing, such as particle agglomeration, large viscosity rebound and other problems. Summary of the invention

[0006] The present application provides a lithium iron manganese phosphate positive electrode sheet and a preparation method thereof, wherein the nano lithium iron manganese phosphate material is grown in situ on a nickel foam current collector by gradually increasing the microwave irradiation power, eliminating the use of a binder, greatly improving the electron transmission path, and the self-supporting nickel foam greatly reduces the agglomeration of the nano lithium iron manganese phosphate material, which is beneficial to the shuttle of lithium ions and constructs a good conductive network. Then, a secondary microwave irradiation hydrothermal acid etching and a tertiary microwave irradiation hydrothermal carbon coating are performed to obtain a lithium iron manganese phosphate positive electrode sheet with excellent performance.

[0007] In a first aspect, a method for preparing a lithium iron manganese phosphate positive electrode sheet is provided, which comprises:

[0008] Adding an iron source, a manganese source, a phosphorus source, a lithium source and a doping element source into a solvent and mixing them to obtain a mixed solution;

[0009] placing nickel foam in the mixed solution for microwave irradiation, and gradually increasing the microwave irradiation power to grow nano-lithium manganese iron phosphate material on the nickel foam;

[0010] Under microwave irradiation, acid-etching the nano-lithium iron manganese phosphate material on the nickel foam to obtain an etched lithium iron manganese phosphate positive electrode sheet;

[0011] The etched lithium iron manganese phosphate positive electrode sheet is transferred to a hydrothermal reactor containing an organic carbon source, and carbon-coated under microwave irradiation to obtain a carbon-coated lithium iron manganese phosphate positive electrode sheet.

[0012] In some embodiments, the microwave irradiation power is increased in a gradient manner, specifically comprising the following steps:

[0013] Adjusting the microwave irradiation power to a first gradient microwave irradiation power so that the mixed solution reacts at 100° C. to 140° C. for 2 min to 5 min;

[0014] The microwave irradiation power is increased to a second gradient microwave irradiation power, so that the mixed solution is reacted at 300° C. to 340° C. for 2 min to 5 min;

[0015] The microwave irradiation power is increased again to a third gradient microwave irradiation power, so that the mixed solution is reacted at 550° C. to 800° C. for 40 min to 60 min.

[0016] In some embodiments, the first gradient microwave irradiation power is 250W to 350W;

[0017] The second gradient microwave irradiation power is 750W to 850W;

[0018] The third gradient microwave irradiation power is 1200W to 1400W.

[0019] In some embodiments, the molar ratio of the iron source to the manganese source is x:(10-x), where x is 1 to 4;

[0020] And / or, the ratio of the molar number of the phosphorus source to the total molar number of the iron source and the manganese source is (1.05-1.2):1;

[0021] And / or, the ratio of the molar number of the lithium source to the total molar number of the iron source and the manganese source is (1.05-1.3):1;

[0022] And / or, the molar number of the doping element source accounts for 0.2% to 1% of the total molar number of the iron source and the manganese source;

[0023] And / or, the added amount of the organic carbon source accounts for 1-10% of the theoretical mass of the carbon-coated lithium manganese iron phosphate material.

[0024] In some embodiments, during acid etching, the microwave irradiation power is adjusted so that the acid etching temperature is 180° C. to 220° C. and the heating time is 25 min to 35 min.

[0025] In some embodiments, during acid etching, the microwave irradiation power is adjusted to 300W-800W.

[0026] In some embodiments, during carbon coating, the microwave irradiation power is adjusted so that the carbon coating temperature is 180° C. to 220° C. and the heating time is 25 min to 35 min.

[0027] In some embodiments, during carbon coating, the microwave irradiation power is adjusted to 400W-600W.

[0028] In some embodiments, the lithium source includes one or more of lithium hydroxide monohydrate and lithium carbonate;

[0029] And / or, the phosphorus source includes one or more of diammonium dihydrogen phosphate and monoammonium sulfate;

[0030] And / or, the iron source includes one or more of ferrous sulfate heptahydrate, ferrous oxalate, ferrous chloride and ferrous nitrate;

[0031] And / or, the manganese source includes one or more of manganese sulfate monohydrate, manganese oxalate, manganese chloride and manganese nitrate;

[0032] And / or, the organic carbon source includes one or more of sucrose, glucose, furfuryl alcohol and soluble starch;

[0033] And / or, the doping element source includes one or more of a magnesium source and a titanium source.

[0034] In a second aspect, a lithium iron manganese phosphate positive electrode sheet is provided, which is prepared by any of the above-described methods for preparing a lithium iron manganese phosphate positive electrode sheet.

[0035] The beneficial effects of the technical solution provided by this application include:

[0036] This application does not require the use of adhesives, but instead grows nano-lithium manganese iron phosphate materials in situ on the current collector nickel foam through microwave irradiation hydrothermal reaction, solving the problem of reduced ion and electronic conductivity caused by the adhesive. In view of the poor intrinsic kinetic performance of lithium manganese iron phosphate, this application grows nano-lithium manganese iron phosphate materials in situ on the current collector, and the current collector adopts a porous nickel foam self-supporting structure, which effectively reduces the agglomeration of nano-lithium manganese iron phosphate materials, is conducive to the shuttling of lithium ions, builds a good conductive network, increases the reaction area of ​​nano-lithium manganese iron phosphate materials and electrolytes, and improves the lithium ion transmission path.

[0037] Compared with the ordinary hydrothermal reaction, the present application adopts microwave irradiation hydrothermal reaction, so that the nano-lithium manganese iron phosphate material crystallizes quickly, the crystal grows rapidly, reduces the mixing of metal ions, and can make the crystal self-growth on the current collector more reliable. The microwave irradiation hydrothermal reaction of the present application is carried out in three steps. The first step is microwave irradiation hydrothermal method to generate nano-lithium manganese iron phosphate material in situ on the current collector; the second step is microwave irradiation hydrothermal method for acid etching modification; the third step is microwave irradiation hydrothermal method for coating carbon layer modification. After the first step of microwave irradiation is completed, the performance of the nano-lithium manganese iron phosphate material is improved by the subsequent two steps of microwave irradiation. The second step of microwave irradiation dissolves part of the lattice of the nano-lithium manganese iron phosphate material due to the acid etching effect, causing the lithium iron phosphate material to be amorphous, thereby improving the lithium ion transmission channel and improving the rate performance. The third step of microwave irradiation is due to carbon coating, so that carbon is uniformly deposited on the surface of the nano-lithium manganese iron phosphate material to improve the overall electronic conductivity of the nano-lithium manganese iron phosphate material, and the carbon coating can reduce the dissolution of metal ions and improve the stability of the nano-lithium manganese iron phosphate material.

[0038] The first step of microwave irradiation in the present application is carried out by gradiently increasing the microwave irradiation power. That is to say, when the nano-lithium manganese iron phosphate material is in situ grown on the current collector, the microwave irradiation power is controlled to increase the irradiation power in a step-by-step manner. The irradiation at low power is mainly to allow the nano-lithium manganese iron phosphate material to nucleate uniformly, and then the irradiation at high power is mainly to allow the nano-lithium manganese iron phosphate material to crystallize uniformly. The step-by-step irradiation can make the internal element distribution of the nano-lithium manganese iron phosphate material more uniform and stable.

[0039] Then, in the second step, microwave irradiation hydrothermal etching, the etching degree can be controlled by controlling the microwave irradiation power. The higher the Mn / Fe molar ratio, the higher the energy density, but the problem that comes with it is that the kinetic performance is worse and the metal dissolution is more serious. In order to cooperate with the acid etching effect in the second step, usually the higher the Mn / Fe ratio, the greater the hydrofluoric acid concentration and microwave power need to be. The kinetic performance can be improved by stronger etching, so that better etching can be achieved. The present application can directly adjust the etching degree of the nano-manganese iron phosphate lithium material by controlling the microwave irradiation power without adjusting the acid content.

[0040] Finally, in the third step, microwave irradiation hydrothermal carbonization was used to synthesize a binder-free lithium manganese iron phosphate positive electrode sheet with excellent performance. This overcomes the defects of nano-lithium manganese iron phosphate materials in practical applications, such as difficult processing, high composite price, and poor intrinsic kinetic performance, and provides a simple and efficient solution for the application of nano-lithium manganese iron phosphate materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0042] Figure 1 A flow chart of a method for preparing a lithium iron manganese phosphate positive electrode sheet provided in an embodiment of the present application;

[0043] Figure 2 XRD comparison diagram of lithium manganese iron phosphate positive electrode materials prepared in Example 1 and Comparative Example 5 of the present application;

[0044] Figure 3 SEM image of unloaded nickel foam provided for this application;

[0045] Figure 4 This is a SEM image of the carbon-coated lithium manganese iron phosphate positive electrode sheet prepared in Example 1 of the present application;

[0046] Figure 5 This is a SEM image of the carbon-coated lithium manganese iron phosphate positive electrode sheet prepared in Comparative Example 1 of the present application;

[0047] Figure 6 This is a SEM image of the carbon-coated lithium manganese iron phosphate positive electrode sheet prepared in Comparative Example 2 of the present application. DETAILED DESCRIPTION

[0048] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0049] See also Figure 1 As shown, the embodiment of the present application provides a method for preparing a lithium manganese iron phosphate positive electrode sheet, which comprises the following steps:

[0050] 101: Add an iron source, a manganese source, a phosphorus source, a lithium source and a doping element source into a solvent, and mix well to obtain a mixed solution.

[0051] Specifically, the iron source and the manganese source are first added to the solvent and mixed evenly, then the phosphorus source and the lithium source are added thereto and mixed evenly, and finally the doping element source is added and the solution is mixed evenly until it becomes clear and transparent.

[0052] Among them, the role of the doping element source is to provide doping element ions, so that when the nano-manganese iron phosphate lithium material is subsequently grown, the volume of a single unit cell is smaller and the channel of the lithium ion transmission path is larger, thereby improving the ion conductivity.

[0053] The molar ratio of the iron source to the manganese source is x:(10-x), where x is 1 to 4. As a preferred example, x=4, and the molar ratio of the iron source to the manganese source is 4:6.

[0054] The ratio of the molar number of the phosphorus source to the total molar number of the iron source and the manganese source is (1.05-1.2):1.

[0055] The ratio of the molar number of the lithium source to the total molar number of the iron source and the manganese source is (1.05-1.3):1.

[0056] The molar number of the doping element source accounts for 0.2% to 1% of the total molar number of the iron source and the manganese source.

[0057] The lithium source includes one or more of lithium hydroxide monohydrate and lithium carbonate;

[0058] The phosphorus source may be a commonly used material. For example, the phosphorus source includes one or more of diammonium dihydrogen phosphate and monoammonium sulfate.

[0059] The iron source may be a commonly used material. For example, the iron source includes one or more of ferrous sulfate heptahydrate, ferrous oxalate, ferrous chloride and ferrous nitrate.

[0060] The manganese source may be a commonly used material. For example, the manganese source includes one or more of manganese sulfate monohydrate, manganese oxalate, manganese chloride and manganese nitrate.

[0061] The doping element source may be made of commonly used materials. For example, the doping element source includes one or more of a magnesium source and a titanium source to provide magnesium ions and titanium ions.

[0062] The magnesium source may be a commonly used material. For example, the magnesium source includes one or more of magnesium chloride (MgCl2), magnesium sulfate (MgSO4), magnesium nitrate (Mg(NO3)2) and magnesium acetate (Mg(CH3COO)2).

[0063] The titanium source may be a commonly used material. For example, the titanium source includes one or more of titanium tetrachloride (TiCl4), tetrabutyl titanate (TBT) and tetraethyl titanate (TEOT).

[0064] The solvent may be water, such as deionized water.

[0065] 102: placing nickel foam in the mixed solution for microwave irradiation, and gradually increasing the microwave irradiation power to grow nano-manganese iron lithium phosphate material on the nickel foam.

[0066] 103: Under microwave irradiation, acid-etching the nano-lithium iron manganese phosphate material on the nickel foam to obtain an etched lithium iron manganese phosphate positive electrode sheet.

[0067] In the present application, a hydrofluoric acid (HF) solution is used for etching, for example, a hydrofluoric acid solution with a concentration of 1 M is used. The advantage of acid etching is that after hydrofluoric acid etching under microwave irradiation, the lithium iron manganese phosphate crystals have defects, and it can be seen from XRD that the crystallinity decreases. After acid etching, the lithium iron manganese phosphate crystals produce more disorder, thereby improving the dynamic performance of the lithium iron manganese phosphate positive electrode sheet.

[0068] 104: The etched lithium iron manganese phosphate positive electrode sheet is transferred to a hydrothermal reactor containing an organic carbon source, and carbon-coated under microwave irradiation to obtain a carbon-coated lithium iron manganese phosphate positive electrode sheet.

[0069] Wherein, the addition amount of the organic carbon source accounts for 1-10% of the theoretical mass of the carbon-coated lithium manganese iron phosphate material.

[0070] It should be noted that the theoretical mass of the carbon-coated lithium manganese iron phosphate material refers to the mass of the carbon-coated lithium manganese iron phosphate material obtained by further calculating the theoretical mass of the uncoated lithium manganese iron phosphate material based on the total molar number of manganese ions and iron ions and the carbon coating amount accounting for 1 to 10% of the total mass of the material.

[0071] It should be noted that in the above step 103, the etched lithium manganese iron phosphate positive electrode sheet includes foamed nickel and the etched nano-lithium manganese iron phosphate material thereon.

[0072] In the above step 104, the carbon-coated lithium manganese iron phosphate positive electrode sheet includes nickel foam and nano-lithium manganese iron phosphate material that has been etched and carbon-coated thereon.

[0073] The carbon-coated lithium iron manganese phosphate material is a nano-lithium iron manganese phosphate material that has been etched and carbon-coated. Compared with the carbon-coated lithium iron manganese phosphate positive electrode sheet in step 104, it lacks foamed nickel.

[0074] The organic carbon source may be a commonly used material. For example, the organic carbon source includes one or more of sucrose, glucose, furfuryl alcohol and soluble starch.

[0075] This application does not require the use of adhesives, but instead grows nano-lithium manganese iron phosphate materials in situ on the current collector nickel foam through microwave irradiation hydrothermal reaction, solving the problem of reduced ion and electronic conductivity caused by the adhesive. In view of the poor intrinsic kinetic performance of lithium manganese iron phosphate, this application grows nano-lithium manganese iron phosphate materials in situ on the current collector, and the current collector adopts a porous nickel foam self-supporting structure, which effectively reduces the agglomeration of nano-lithium manganese iron phosphate materials, is conducive to the shuttling of lithium ions, builds a good conductive network, increases the reaction area of ​​nano-lithium manganese iron phosphate materials and electrolytes, and improves the lithium ion transmission path.

[0076] Compared with the ordinary hydrothermal reaction, the present application adopts microwave irradiation hydrothermal reaction, so that the nano-manganese iron lithium phosphate material crystallizes quickly, the crystal grows rapidly, reduces the mixing of metal ions, and can make the crystal self-growth on the current collector more reliable. The microwave irradiation hydrothermal reaction of the present application is carried out in three steps. The first step is microwave irradiation hydrothermal method to generate nano-manganese iron lithium phosphate material in situ on the current collector; the second step is microwave irradiation hydrothermal method for acid etching modification; the third step is microwave irradiation hydrothermal method for coating carbon layer modification. After the first step of microwave irradiation synthesis is completed, the performance of the nano-manganese iron lithium phosphate material is improved by the subsequent two steps of microwave irradiation. The second step of microwave irradiation dissolves part of the lattice of the nano-manganese iron lithium phosphate material due to the acid etching effect, causing the material to be amorphous, thereby improving the lithium ion transmission channel and improving the rate performance. The third step of microwave irradiation is due to carbon coating, so that carbon is uniformly deposited on the surface of the nano-manganese iron lithium phosphate material to improve the overall electronic conductivity of the nano-manganese iron lithium phosphate material, and the carbon coating can reduce the dissolution of metal ions and improve the stability of the nano-manganese iron lithium phosphate material.

[0077] In addition, the first step of microwave irradiation in the present application is carried out by gradiently increasing the microwave irradiation power. That is to say, when the nano-lithium manganese iron phosphate material is in situ grown on the current collector, the microwave irradiation power is controlled to increase the irradiation power in steps. The irradiation at low power is mainly to allow the nano-lithium manganese iron phosphate material to nucleate uniformly, and then the irradiation at high power is mainly to allow the nano-lithium manganese iron phosphate material to crystallize uniformly. The step irradiation can make the internal element distribution of the nano-lithium manganese iron phosphate material more uniform and stable.

[0078] Then, in the second step, microwave irradiation hydrothermal etching, the etching degree can be controlled by controlling the microwave irradiation power. The higher the Mn / Fe molar ratio, the higher the energy density, but the problem that comes with it is that the kinetic performance is worse and the metal dissolution is more serious. In order to cooperate with the acid etching effect in the second step, usually the higher the Mn / Fe ratio, the greater the hydrofluoric acid concentration and microwave power need to be. The kinetic performance can be improved by stronger etching, so that better etching can be achieved. The present application can directly adjust the etching degree of the nano-manganese iron phosphate lithium material by controlling the microwave irradiation power without adjusting the acid content.

[0079] Finally, in the third step, microwave irradiation hydrothermal carbonization was used to synthesize a binder-free lithium manganese iron phosphate positive electrode sheet with excellent performance. This overcomes the defects of nano-lithium manganese iron phosphate materials in practical applications, such as difficult processing, high composite price, and poor intrinsic kinetic performance, and provides a simple and efficient solution for the application of nano-lithium manganese iron phosphate materials.

[0080] In the above step 102, the microwave irradiation power is gradually increased, which specifically includes the following steps:

[0081] 201: Adjusting the microwave irradiation power to a first gradient microwave irradiation power, so that the mixed solution reacts at 100° C. to 140° C. for 2 min to 5 min.

[0082] In step 201, in order to control the reaction temperature of the mixed solution by microwave irradiation, the first gradient microwave irradiation power in the present application is 250W to 350W, so as to reach 100°C to 140°C.

[0083] 202: increasing the microwave irradiation power to a second gradient microwave irradiation power, so that the mixed solution reacts at 300° C. to 340° C. for 2 min to 5 min.

[0084] In step 202, in order to control the reaction temperature of the mixed solution by microwave irradiation, the second gradient microwave irradiation power in the present application is 750W to 850W, so as to reach 300°C to 340°C.

[0085] 203: increasing the microwave irradiation power again to a third gradient microwave irradiation power, so that the mixed solution reacts at 550° C. to 800° C. for 40 min to 60 min.

[0086] In step 203, in order to control the reaction temperature of the mixed solution by microwave irradiation, the third gradient microwave irradiation power in the present application is 1200W-1400W, so as to reach 550°C-800°C.

[0087] By increasing the microwave irradiation power in a gradient manner, a slow gradient temperature rise is achieved, so that the mixed solution can be mixed more evenly, so that the lithium iron manganese phosphate can be evenly spread on the nickel foam during the nucleation process. Specifically, under the first gradient microwave irradiation power of step 201, all ions in the mixed solution can be mixed more evenly, under the second gradient microwave irradiation power of step 202, the lithium iron manganese phosphate can be uniformly nucleated, and under the third gradient microwave irradiation power of step 203, the lithium iron manganese phosphate crystals can be uniformly grown. It should be noted that the irradiation under the first gradient microwave irradiation power of step 201 and the irradiation under the second gradient microwave irradiation power of step 202 are irradiations at low power, and the irradiation under the third gradient microwave irradiation power of step 203 is irradiation at high power.

[0088] In the process of gradient increasing the microwave irradiation power, if the microwave irradiation power is too high, the crystal particles of the lithium iron manganese phosphate material will become larger. On the one hand, the larger particles will make the lithium ion transmission path longer, which will lead to a decrease in the rate performance of the battery; on the other hand, the larger particles will cause the body impedance of the lithium iron manganese phosphate material to increase and the power loss to increase, which will cause a slight decrease in the cycle performance of the battery; if the microwave irradiation power is too low, the crystallinity of the lithium iron manganese phosphate material will decrease, which will lead to a decrease in the cycle performance and rate performance of the battery.

[0089] If high temperature conditions are used directly for the reaction, the nano-manganese iron phosphate lithium material will be locally aggregated, and the locally aggregated nano-manganese iron phosphate lithium material will not be in sufficient contact with the electrolyte, resulting in poor rate performance of the battery.

[0090] In the above step 103, during acid etching, the microwave irradiation power is adjusted so that the acid etching temperature is 180° C. to 220° C. and the heating time is 25 min to 35 min.

[0091] Specifically, in order to control the temperature of acid etching by microwave irradiation, during acid etching, the microwave irradiation power is adjusted to 300W to 800W in the present application, so as to reach 180°C to 220°C.

[0092] During the acid etching process, if the microwave irradiation power is too high, the nano-lithium manganese iron phosphate material will be over-etched, aggravating the dissolution of transition metal ions, thereby slightly reducing the cycle performance of the battery; if the microwave irradiation power is too low, the nano-lithium manganese iron phosphate material will be insufficiently etched, resulting in no obvious improvement in the battery's rate performance.

[0093] In the above step 104, during carbon coating, the microwave irradiation power is adjusted so that the carbon coating temperature is 180° C. to 220° C. and the heating time is 25 min to 35 min.

[0094] Specifically, in order to control the temperature of carbon coating by microwave irradiation, during carbon coating, the microwave irradiation power is adjusted to 400W-600W in the present application, so as to reach 180°C-220°C.

[0095] During the carbon coating process, if the microwave irradiation power is too high, the carbon layer coating thickness will be too large, resulting in a slight decrease in the battery's rate performance; if the microwave irradiation power is too low, the dissolution of transition metal ions will be slightly serious, resulting in a slight decrease in the battery's cycle performance.

[0096] The invention is described in detail below through several embodiments and comparative examples.

[0097] Example 1

[0098] Step 1: Mix a lithium source, a phosphorus source, an iron source, a manganese source and a doping element source into a solution, and transfer the solution to a microwave irradiation reactor.

[0099] Specifically, ferrous sulfate heptahydrate and manganese sulfate monohydrate are mixed in deionized water, and the molar ratio of ferrous sulfate heptahydrate to manganese sulfate monohydrate is 4:6; then diammonium phosphate and lithium hydroxide monohydrate are added, wherein the molar ratio of diammonium phosphate to the total molar number of ferrous sulfate heptahydrate and manganese sulfate monohydrate is 1.20:1, and the molar ratio of lithium hydroxide monohydrate to the total molar number of ferrous sulfate heptahydrate and manganese sulfate monohydrate is 1.23:1. Finally, a doping element source is added, and the doping element source is magnesium sulfate (MgSO4) and titanium tetrachloride (TiCl4) with a molar ratio of 4:1, and the molar number of the doping element source accounts for 0.5% of the total molar number of ferrous sulfate heptahydrate and manganese sulfate monohydrate, and the solution is mixed evenly until it is clear and transparent.

[0100] Step 2: Place the commercial nickel foam vertically into the solution and perform microwave irradiation in a sealed state by gradiently increasing the microwave irradiation power.

[0101] Specifically, the microwave irradiation power is first adjusted to a first gradient microwave irradiation power of 300 W, and the irradiation is performed for 3 minutes. At this power, the reaction temperature is 100° C. to 140° C.

[0102] Then the microwave irradiation power was adjusted to the second gradient microwave irradiation power of 800W, and the irradiation was performed for 3 minutes. At this power, the reaction temperature was 300°C to 340°C.

[0103] Finally, the microwave irradiation power was adjusted to the third gradient microwave irradiation power of 1300W to form a high-temperature and high-pressure aqueous solution, and the reaction was carried out by ion diffusion for 40 minutes to grow nano-manganese iron lithium phosphate material on the nickel foam. At this power, the reaction temperature reached the calcination temperature of 550°C to 800°C.

[0104] Step 3: After washing and drying, transfer to a 1M hydrofluoric acid solution and perform a secondary microwave irradiation hydrothermal reaction. The given power is 500W, and the reaction temperature is controlled at 180°C to 220°C. After irradiation heating for 30 minutes, an etched lithium manganese iron phosphate positive electrode sheet is obtained.

[0105] Step 4: After washing and drying, transfer to a hydrothermal reactor containing an organic carbon source, perform three microwave irradiation hydrothermal reactions, set the power at 500 W, control the reaction temperature at 180°C to 220°C, irradiate and heat for 30 minutes, and finally obtain a carbon-coated lithium manganese iron phosphate positive electrode sheet.

[0106] Example 2

[0107] The difference between Example 2 and Example 1 is that:

[0108] When the microwave irradiation power is gradually increased in step 2, the microwave irradiation power is first adjusted to a first gradient microwave irradiation power of 250 W, then adjusted to a second gradient microwave irradiation power of 750 W, and finally adjusted to a third gradient microwave irradiation power of 1200 W.

[0109] The microwave irradiation power during etching in step 3 is 300W.

[0110] The microwave irradiation power during carbon coating in step 4 is 400W.

[0111] Example 3

[0112] The difference between Example 3 and Example 1 is that:

[0113] When the microwave irradiation power is gradually increased in step 2, the microwave irradiation power is first adjusted to a first gradient microwave irradiation power of 350 W, then adjusted to a second gradient microwave irradiation power of 850 W, and finally adjusted to a third gradient microwave irradiation power of 1400 W.

[0114] The microwave irradiation power during etching in step 3 is 800W.

[0115] The microwave irradiation power during carbon coating in step 4 is 600W.

[0116] Example 4

[0117] The difference between Example 4 and Example 1 is that the molar ratio of ferrous sulfate heptahydrate to manganese sulfate monohydrate in step 1 is 1:9.

[0118] Embodiment 5:

[0119] The difference between Example 5 and Example 1 is that when the microwave irradiation power is gradually increased in step 2, the microwave irradiation power is first adjusted to a first gradient microwave irradiation power of 200 W, then the microwave irradiation power is adjusted to a second gradient microwave irradiation power of 700 W, and finally the microwave irradiation power is adjusted to a third gradient microwave irradiation power of 1100 W.

[0120] Embodiment 6:

[0121] The difference between Example 6 and Example 1 is that when the microwave irradiation power is gradually increased in step 2, the microwave irradiation power is first adjusted to a first gradient microwave irradiation power of 400 W, then the microwave irradiation power is adjusted to a second gradient microwave irradiation power of 900 W, and finally the microwave irradiation power is adjusted to a third gradient microwave irradiation power of 1500 W.

[0122] Embodiment 7:

[0123] The difference between Example 7 and Example 1 is that the etching power in step 3 is 200W.

[0124] Embodiment 8:

[0125] The difference between Example 8 and Example 1 is that the etching power in step 3 is 900W.

[0126] Comparative Example 1:

[0127] The difference between Comparative Example 1 and Example 1 is that step 2 only includes the first gradient microwave irradiation power and the second gradient microwave irradiation power, but does not include the third gradient microwave irradiation power.

[0128] Comparative Example 2:

[0129] The difference between Comparative Example 2 and Example 1 is that step 2 only includes the third gradient microwave irradiation power, and does not include the first gradient microwave irradiation power and the second gradient microwave irradiation power.

[0130] Comparative Example 3:

[0131] The difference between Comparative Example 3 and Example 4 is that step 2 only includes the first gradient microwave irradiation power and the second gradient microwave irradiation power, but does not include the third gradient microwave irradiation power.

[0132] Comparative Example 4:

[0133] The difference between Comparative Example 4 and Example 4 is that step 2 only includes the third gradient microwave irradiation power, and does not include the first gradient microwave irradiation power and the second gradient microwave irradiation power.

[0134] Comparative Example 5:

[0135] The difference between Comparative Example 5 and Example 1 is that step 3 is not included, that is, the acid etching step is not performed.

[0136] Battery preparation:

[0137] Graphite PQ2-X13 (purchased from Hunan Zhongke Xingcheng), binder (PVDF), and conductive carbon (SP) were homogenized and stirred in a mass ratio of 96%: 2%: 2% and then coated on copper foil to form a negative electrode sheet. The compaction density of the negative electrode sheet was set to 1.58g / cc. The diaphragm used RPH2186 (purchased from Shanghai Enjie) and the electrolyte used LBC-410A03 (purchased from Xinzhoubang). The lithium manganese iron phosphate positive electrode sheet, negative electrode sheet and diaphragm prepared in the above embodiments and comparative examples were assembled into a soft-pack single-laminate battery, and the electrolyte was injected to obtain a lithium-ion battery.

[0138] Performance Test:

[0139] XRD test: using an x-ray diffractometer (Empyrean, Malvern Panalytical) to determine the crystal structure of the lithium iron manganese phosphate positive electrode material on the lithium iron manganese phosphate positive electrode sheet prepared in the above examples and comparative examples, specifically, the lithium iron manganese phosphate positive electrode material was scraped off from the lithium iron manganese phosphate positive electrode sheet with a scraper for collection, and then 0.5 g of the scraped lithium iron manganese phosphate positive electrode material was placed on the sample table of the equipment, and the equipment parameters were set to be within the 2θ range of 15-80°, the scanning speed was 5 degrees / min, and the step size was 0.02 to test and obtain the XRD curve.

[0140] SEM test: A field emission scanning electron microscope (SEM) Carl Zeiss Sigma 300 device was used to observe the morphology of the lithium iron manganese phosphate positive electrode sheets prepared in the above embodiments and comparative examples. Specifically, the lithium iron manganese phosphate positive electrode sheets to be observed were cut into 5mm*5mm pieces and placed on the sample stage of the device. The device parameters were set to observe the surface morphology of the lithium iron manganese phosphate positive electrode sheets at a voltage of 5kV and magnifications of 500 and 2000.

[0141] Test of 0.1C gram capacity: Taking 170mAh / g as the theoretical gram capacity, the mass of the lithium iron manganese phosphate positive electrode sheet prepared in the above embodiments and comparative examples minus the mass of the collector nickel foam is the mass of the lithium iron manganese phosphate positive electrode material. The theoretical capacity is calculated according to the theoretical gram capacity and the mass of the lithium iron manganese phosphate positive electrode material. The current constant capacity is designed to be 0.1C using the theoretical capacity. Then, it is charged to 4.25V at 0.1C, and then discharged to 2.5V at 0.1C. After three cycles, the 0.1C gram capacity at the third cycle is taken.

[0142] Test of 2C gram capacity utilization: 0.33C charge to 4.25V, then 0.33C discharge to 2.5V, after three cycles, take the capacity of the third cycle as the calibration capacity, 0.33C charge to 4.25V, then 2C discharge to 2.5V; the mass of the lithium iron manganese phosphate positive electrode sheet prepared in the above embodiments and comparative examples minus the mass of the collector nickel foam is the mass of the lithium iron manganese phosphate positive electrode material, and the 2C gram capacity utilization is calculated by the 2C discharge capacity and the mass of the lithium iron manganese phosphate positive electrode material.

[0143] Test of 0.5C cycle 200-cycle retention rate: Charge to 4.25V at 0.5C, then discharge to 2.5V at 0.5C, this is one cycle, a total of 200 cycles are performed, and the 0.5C cycle 200-cycle retention rate is obtained by dividing the discharge capacity after 200 cycles by the discharge capacity of the first cycle.

[0144] Metal manganese dissolution test on the negative electrode side: A lithium ion battery was prepared using the lithium iron manganese phosphate positive electrode sheet prepared in the above embodiments and comparative examples. The SOC state of the fresh lithium ion battery was 100%. The lithium ion battery was disassembled in a glove box and the negative electrode sheet was taken out; about 0.35 g of graphite negative electrode powder was taken from the coating area of ​​the negative electrode sheet, and aqua regia and 8 ml of pure water were added in a volume ratio of 2:6. A clean watch glass was covered and placed on a graphite heating plate, and heated at 200°C for 30 min until completely dissolved; the sample was removed and cooled to room temperature, fixed to a 100 ml volumetric flask, deionized water was added and shaken, and the filtrate was taken with a disposable syringe and a 0.45 needle filter for ICP test to obtain the metal manganese dissolution concentration on the negative electrode side.

[0145] See also Figure 2 As shown, it is an XRD comparison diagram of the lithium iron manganese phosphate positive electrode material prepared in Example 1 and Comparative Example 5. It can be seen from the figure that the unetched lithium iron manganese phosphate positive electrode material (Comparative Example 5) is compared with the etched lithium iron manganese phosphate positive electrode material (Example 1). After etching, the crystallinity of the lithium iron manganese phosphate positive electrode material decreases and the disorder increases, thereby improving the kinetic performance of lithium ions.

[0146] See also Figure 3 Shown is the SEM image of unloaded nickel foam.

[0147] See also Figure 4 , which is a SEM image of the carbon-coated lithium iron manganese phosphate positive electrode sheet prepared in Example 1, it can be seen that the lithium iron manganese phosphate crystals grow evenly on the nickel foam.

[0148] See also Figure 5As shown, it is a SEM image of the carbon-coated lithium iron manganese phosphate positive electrode sheet prepared in Comparative Example 1. Since only low-power microwave irradiation, that is, the first gradient microwave irradiation power and the second gradient microwave irradiation power are irradiated, and high-power microwave irradiation is not performed, the crystallization temperature of the lithium iron manganese phosphate material is not reached, resulting in difficulty in the crystallization of lithium iron manganese phosphate. Figure 5 The middle surface is relatively smooth.

[0149] See also Figure 6 As shown, it is an SEM image of the carbon-coated lithium iron manganese phosphate positive electrode sheet prepared in Comparative Example 2. Since only high-power microwave irradiation, i.e., the third gradient microwave irradiation power is used for irradiation, and low-power microwave irradiation is not performed, the uniform nucleation process of the lithium iron manganese phosphate material is lacking, and therefore the lithium iron manganese phosphate crystals will agglomerate locally in the nickel foam collector.

[0150] Table 1

[0151]

[0152] It can be seen from Table 1 that in Examples 1 to 8, the secondary battery further prepared from the lithium manganese iron phosphate positive electrode sheet prepared by the preparation method of the lithium manganese iron phosphate positive electrode sheet provided by the present invention has excellent rate performance and cycle stability, and the dissolution of metallic manganese on the negative electrode side is also low.

[0153] It should be noted that the molar ratio of ferrous sulfate heptahydrate to manganese sulfate monohydrate in Example 4 is 1:9, and the molar ratio of ferrous sulfate heptahydrate to manganese sulfate monohydrate in Example 1 is 4:6. Therefore, relative to Example 1, the manganese content in Example 4 is higher, so the dissolution of metallic manganese on the negative electrode side is more serious; in addition, due to the high manganese content, a more serious Jan-Taylor effect will occur, resulting in a decrease in the rate performance and cycle performance of the battery.

[0154] In combination with Example 1, Example 5 and Example 6, during the process of gradient increasing the microwave irradiation power, if the microwave irradiation power is too high, the crystal particles of the lithium iron manganese phosphate material will become larger. On the one hand, the increase in particles will make the lithium ion transmission path longer, which will cause the battery's rate performance to decrease; on the other hand, the increase in particles will cause the body impedance of the lithium iron manganese phosphate material to increase, and the power loss to increase, which will cause the battery's cycle performance to slightly decrease; if the microwave irradiation power is too low, the crystallinity of the lithium iron manganese phosphate material will decrease, which will cause the battery's cycle performance and rate performance to decrease.

[0155] In combination with Example 1, Example 7 and Example 8, during the acid etching process, if the microwave irradiation power is too high, the nano-lithium manganese iron phosphate material will be over-etched, aggravating the dissolution of transition metal ions, thereby causing a slight decrease in the cycle performance of the battery; if the microwave irradiation power is too low, the nano-lithium manganese iron phosphate material will be insufficiently etched, resulting in an insignificant improvement in the rate performance of the battery.

[0156] In combination with Example 1 and Comparative Example 1 and Comparative Example 2, and in combination with Example 4 and Comparative Example 3 and Comparative Example 4, since only low-power microwave irradiation was performed in Comparative Example 1 and Comparative Example 3, and no high-power microwave irradiation was performed, it was difficult for the lithium iron manganese phosphate material to crystallize and grow uniformly after nucleation, so the rate performance of the battery prepared therefrom was very poor. In Comparative Example 2 and Comparative Example 4, only high-power microwave irradiation was performed, and no low-power microwave irradiation was performed. Although the lithium iron manganese phosphate material lacked a uniform nucleation process, lithium iron manganese phosphate crystals still appeared. However, due to the local agglomeration of crystals in the nickel foam current collector, the rate performance of the battery prepared therefrom was reduced.

[0157] In combination with Example 1 and Comparative Example 5, since hydrofluoric acid etching is performed in Example 1, part of the crystal lattice of the nano-lithium manganese iron phosphate material is dissolved to cause the material to become amorphous, thereby improving the lithium ion transmission channel and improving the rate performance of the battery prepared therefrom. However, hydrofluoric acid etching is not performed in Comparative Example 5, and the rate performance of the battery prepared therefrom is reduced.

[0158] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for preparing a lithium manganese iron phosphate positive electrode sheet, It is characterized in that It includes: Adding an iron source, a manganese source, a phosphorus source, a lithium source and a doping element source into a solvent and mixing them to obtain a mixed solution; placing nickel foam in the mixed solution for microwave irradiation, and gradually increasing the microwave irradiation power to grow nano-lithium manganese iron phosphate material on the nickel foam; Under microwave irradiation, acid-etching the nano-lithium iron manganese phosphate material on the nickel foam to obtain an etched lithium iron manganese phosphate positive electrode sheet; The etched lithium iron manganese phosphate positive electrode sheet is transferred to a hydrothermal reactor containing an organic carbon source, and carbon-coated under microwave irradiation to obtain a carbon-coated lithium iron manganese phosphate positive electrode sheet.

2. The method for preparing the lithium iron manganese phosphate positive electrode sheet according to claim 1, It is characterized in that Gradiently increasing the microwave irradiation power specifically includes the following steps: Adjusting the microwave irradiation power to a first gradient microwave irradiation power so that the mixed solution reacts at 100° C. to 140° C. for 2 min to 5 min; The microwave irradiation power is increased to a second gradient microwave irradiation power, so that the mixed solution is reacted at 300° C. to 340° C. for 2 min to 5 min; The microwave irradiation power is increased again to a third gradient microwave irradiation power, so that the mixed solution is reacted at 550° C. to 800° C. for 40 min to 60 min.

3. The method for preparing the lithium iron manganese phosphate positive electrode sheet according to claim 2, Features: The first gradient microwave irradiation power is 250W to 350W; The second gradient microwave irradiation power is 750W to 850W; The third gradient microwave irradiation power is 1200W to 1400W.

4. The method for preparing the lithium iron manganese phosphate positive electrode sheet according to claim 1, Features: The molar ratio of the iron source to the manganese source is x:(10-x), where x is 1 to 4; And / or, the ratio of the molar number of the phosphorus source to the total molar number of the iron source and the manganese source is (1.05-1.2):1; And / or, the ratio of the molar number of the lithium source to the total molar number of the iron source and the manganese source is (1.05-1.3):1; And / or, the molar number of the doping element source accounts for 0.2% to 1% of the total molar number of the iron source and the manganese source; And / or, the added amount of the organic carbon source accounts for 1-10% of the theoretical mass of the carbon-coated lithium manganese iron phosphate material.

5. The method for preparing the lithium iron manganese phosphate positive electrode sheet according to claim 1, Features: During acid etching, the microwave irradiation power is adjusted so that the acid etching temperature is 180° C. to 220° C. and the heating time is 25 min to 35 min.

6. The method for preparing the lithium iron manganese phosphate positive electrode sheet according to claim 5, Features: During acid etching, adjust the microwave irradiation power to 300W-800W.

7. The method for preparing the lithium iron manganese phosphate positive electrode sheet according to claim 1, Features: During carbon coating, the microwave irradiation power is adjusted so that the carbon coating temperature is 180° C. to 220° C. and the heating time is 25 min to 35 min.

8. The method for preparing the lithium iron manganese phosphate positive electrode sheet according to claim 7, Features: During carbon coating, the microwave irradiation power was adjusted to 400W-600W.

9. The method for preparing the lithium iron manganese phosphate positive electrode sheet according to claim 1, Features: The lithium source includes one or more of lithium hydroxide monohydrate and lithium carbonate; And / or, the phosphorus source includes one or more of diammonium dihydrogen phosphate and monoammonium sulfate; And / or, the iron source includes one or more of ferrous sulfate heptahydrate, ferrous oxalate, ferrous chloride and ferrous nitrate; And / or, the manganese source includes one or more of manganese sulfate monohydrate, manganese oxalate, manganese chloride and manganese nitrate; And / or, the organic carbon source includes one or more of sucrose, glucose, furfuryl alcohol and soluble starch; And / or, the doping element source includes one or more of a magnesium source and a titanium source.

10. A lithium manganese iron phosphate positive electrode sheet, Features: It is prepared by the method for preparing a lithium manganese iron phosphate positive electrode sheet as described in any one of claims 1 to 9.