Preparation method of composite positive electrode material, composite positive electrode material and solid-state battery
By using ball milling dispersion and high-temperature inert gas drying in the preparation method, the problem of uneven distribution of solid electrolyte in the positive electrode material of all-solid-state batteries was solved, thereby improving the energy density of the battery.
Patent Information
- Application Number
- CN202411386496.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-29
AI Technical Summary
The uneven distribution of solid electrolyte and the low proportion of active material in existing all-solid-state battery cathode materials result in low energy density, which limits their application.
A composite positive electrode material is prepared by obtaining a pre-prepared mixed solution containing positive electrode active material, solid electrolyte, conductive carbon and solvent, dispersing it and then drying it with an inert gas. The specific steps include ball milling dispersion and high-temperature inert gas drying.
This increases the contact points between the solid electrolyte and the positive electrode active material, reduces the obstruction of lithium-ion migration, and improves the energy density of the battery.
Smart Images

Figure CN119050332A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery materials, and in particular to a method for preparing a composite positive electrode material, the composite positive electrode material and a solid-state battery. Background Art
[0002] Although traditional lithium-ion batteries are widely used in the electronics field and have the advantage of high energy density, they have great safety hazards due to problems such as electrolyte leakage and thermal runaway. All-solid-state batteries are a solution that uses solid electrolytes instead of electrolytes and uses solid electrolytes as lithium ion transmission channels. It avoids the safety hazards of lithium-ion batteries and has become a current research hotspot.
[0003] In the prior art, since all-solid-state electrolytes are batteries that use solid electrolytes instead of electrolytes, how to achieve rapid lithium ion migration inside the battery becomes the key to the practical application of all-solid-state batteries. However, the positive electrode of existing solid-state batteries is usually directly mixed with solid electrolytes and positive electrode active materials and then directly dried, which easily causes problems such as uneven distribution of solid electrolytes and low proportion of positive electrode active materials, resulting in low energy density of all-solid-state batteries, limiting their application. Summary of the invention
[0004] In order to solve the above technical problems, the present application discloses, on one hand, a method for preparing a composite positive electrode material, which comprises:
[0005] Obtaining a preset mixed solution; the preset mixed solution contains a positive electrode active material, a solid electrolyte, conductive carbon and a solvent;
[0006] Performing a dispersion process on the preset mixed solution to obtain a target mixture;
[0007] An inert gas is introduced into the target mixture, and then a drying process is performed to obtain a composite positive electrode material.
[0008] Furthermore, the temperature of the introduced inert gas is 50°C to 700°C.
[0009] Furthermore, the inert gas has an inlet flow rate of 10 m / s to 30 m / s;
[0010] The inert gas is introduced for a time of 1 second to 30 seconds.
[0011] Furthermore, the dispersing treatment of the preset mixed solution to obtain the target mixture includes:
[0012] The preset mixed solution is dispersed by using a ball mill to obtain a target mixture.
[0013] Furthermore, in the dispersion process, the ball-to-material ratio in the ball mill is 1:1 to 20:1.
[0014] Furthermore, the chemical formula of the solid electrolyte is (100-xy)Li2S·xP2S5·yM m N n , wherein 0≤x<100, 0≤y<100, 0≤x+y<100, 0≤m<4, 0≤n<6, M is one or more of Li, Ge, Si, Sn, Sb, and N is at least one of Se, O, Cl, Br, and I;
[0015] The positive electrode active material includes at least one of lithium iron phosphate, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel manganese oxide, lithium-rich manganese-based oxide material, lithium manganese iron phosphate, lithium cobalt oxide and lithium manganese oxide;
[0016] The conductive carbon comprises at least one of Super P, carbon nanotubes, Ketjen black, carbon fiber, graphene and acetylene black;
[0017] The solvent includes at least one of esters, ethers, ketones and alkanes.
[0018] Furthermore, the mass ratio of the positive electrode active material, the solid electrolyte and the conductive carbon is (90-98):(9-1):1.
[0019] Furthermore, the solid content of the preset mixed solution is 10% to 70%.
[0020] On the other hand, the present application discloses a composite positive electrode material, which is prepared based on the above-mentioned preparation method.
[0021] The present application discloses a solid-state battery in another aspect, wherein the positive electrode of the solid-state battery adopts the above-mentioned composite positive electrode material.
[0022] Using the above technical solution, the preparation method of the composite positive electrode material provided in this application has the following characteristics:
[0023] Beneficial effects:
[0024] The embodiment of the present application obtains a preset mixed solution (specifically comprising a positive electrode active material, a solid electrolyte, conductive carbon and a solvent), first disperses the preset mixed solution, and then sequentially introduces an inert gas and performs a drying process, thereby speeding up the removal of the solvent in the solution and reducing the drying time, thereby avoiding problems such as excessive particle size growth of the solid electrolyte in the solution during the drying process, reducing the contact points with the positive electrode active material and hindering the migration of lithium ions, and can greatly improve the energy density of the battery using it. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0026] Figure 1 is a schematic diagram of an exemplary process for preparing a composite positive electrode material;
[0027] Figure 2 is a scanning electron microscope image corresponding to an exemplary embodiment 1;
[0028] Figure 3 The following is a scanning electron microscope image corresponding to an exemplary comparative example 1. DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0030] The term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure or characteristic that may be included in at least one implementation of the present application. In the description of the present application, it should be understood that the orientation or positional relationship indicated by the terms "upper", "lower", "top", "bottom", etc. is based on the orientation or positional relationship shown in the accompanying drawings, which is only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present application. In addition, the terms "first" and "second" are used only for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may include one or more of the features explicitly or implicitly. Moreover, the terms "first", "second", etc. are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments of the present application described here can be implemented in an order other than those illustrated or described here.
[0031] For the purpose of the following detailed description, it should be understood that the present invention may adopt various alternative changes and step sequences, unless expressly specified to the contrary. In addition, except in any operating examples, or otherwise indicated, all numbers representing the amount of ingredients used in the specification and claims should be understood to be modified by the term "about" in all cases. Therefore, unless otherwise indicated, the numerical parameters set forth in the following specification and the attached claims are approximate values that vary according to the desired performance to be obtained by the present invention. At least it is not intended to limit the application of the doctrine of equivalents to the scope of the claims, and each numerical parameter should at least be interpreted according to the number of reported significant figures and by applying ordinary rounding techniques.
[0032] Notwithstanding that the numerical ranges and parameters setting forth the broad scope of the invention are approximations, the numerical values set forth in the specific examples are reported as precisely as possible. Any numerical value, however, inherently contains certain errors necessarily resulting from the standard deviation found in their respective testing measurements.
[0033] When a numerical range is disclosed herein, the above range is deemed to be continuous and includes the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all sub-ranges included therein. For example, a specified range from "1 to 10" should be deemed to include any and all sub-ranges between a minimum of 1 and a maximum of 10. Exemplary sub-ranges of ranges 1 to 10 include, but are not limited to, 1 to 6.1, 3.5 to 7.8, 5.5 to 10, etc.
[0034] See also Figure 1 , which is a schematic flow chart of an exemplary method for preparing a composite positive electrode material. The method for preparing a composite positive electrode material provided may specifically include:
[0035] S101: Obtaining a preset mixed solution; the preset mixed solution contains a positive electrode active material, a solid electrolyte, conductive carbon and a solvent.
[0036] In the embodiments of the present application, the positive electrode active material, the solid electrolyte, the conductive carbon and the solvent may be premixed in a certain ratio.
[0037] In an exemplary embodiment, the mass ratio of the positive electrode active material, the solid electrolyte and the conductive carbon is (90-98): (9-1): 1. In other words, when the mass fraction of the conductive carbon is 1 part, the mass fraction of the positive electrode active material is 90 to 98 parts. Specifically, the mass fraction of the positive electrode active material can be 90 parts, 91 parts, 92 parts, 93 parts, 94 parts, 95 parts, 96 parts, 97 parts or 98 parts, and the mass fraction of the solid electrolyte is 1 to 9 parts. Specifically, the mass fraction of the solid electrolyte can be 1 part, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts or 9 parts. For example, the mass ratio of the positive electrode active material, the solid electrolyte and the conductive carbon can be 98:1; 1, 90:9:1, 94:5:1.
[0038] In an exemplary embodiment, the solid content of the preset mixed solution is 10% to 70%, such as 10%, 20%, 30%, 40%, 50%, 60% or 70%. In order to achieve a better coating effect, the solid content of the preset mixed solution is 20% to 50%.
[0039] In an exemplary embodiment, the solid electrolyte may be a sulfide having a room temperature lithium ion conductivity comparable to that of a conventional electrolyte (>1×10 -3 S cm -1 ), which can be used as an ion mediator to construct a composite positive electrode. The chemical formula of the solid electrolyte is (100-xy)Li2S·xP2S5·yM m N n , wherein 0≤x<100, 0≤y<100, 0≤x+y<100, 0≤m<4, 0≤n<6, M is one or more of Li, Ge, Si, Sn, Sb, and N is at least one of Se, O, Cl, Br, and I.
[0040] In an exemplary embodiment, the positive electrode active material includes at least one of lithium iron phosphate (hereinafter referred to as LFP), lithium nickel cobalt manganese oxide (hereinafter referred to as NCM), lithium nickel cobalt aluminum oxide (hereinafter referred to as NCA), lithium nickel manganese oxide (hereinafter referred to as LNMO), lithium-rich manganese-based oxide material (hereinafter referred to as LRMO), lithium manganese iron phosphate (hereinafter referred to as LMP), lithium cobalt oxide (hereinafter referred to as LCO), and lithium manganese oxide (hereinafter referred to as LMO).
[0041] In an exemplary embodiment, the conductive carbon includes at least one of Super P, carbon nanotubes, Ketjen black, carbon fiber, graphene and acetylene black;
[0042] In an exemplary embodiment, the solvent includes at least one of esters, ethers, ketones and alkanes.
[0043] S102: performing a dispersion process on the preset mixed solution to obtain a target mixture.
[0044] In an exemplary embodiment, the step S102 of dispersing the preset mixed solution to obtain the target mixture includes: dispersing the preset mixed solution using a ball mill to obtain the target mixture. In this way, the target mixture is dispersed using a ball mill, and the electrolyte can be refined to the nanometer level, and the effect of uniform coating on the surface of the positive electrode active material is achieved.
[0045] In the embodiment of the present application, in the dispersion process, the ball-to-material ratio in the ball mill is 1:1 to 20:1. That is, the mass ratio of the ball milled to the target mixture is 1:1 to 20:1. Specifically, the ball-to-material ratio in the ball mill is 1:1, 5:1, 10:1, 15:1 or 20:1. Optionally, in order to achieve a better dispersion effect, the ball-to-material ratio is 10:1. The ball milling time is 1 to 50h, specifically, the ball milling time is 1h, 5h, 10h, 15h, 20h, 25h, 30h, 35h, 40h, 45h or 50h. In order to achieve a better dispersion effect, the ball milling time can be 5h. Optionally, the ball milling speed is 100 to 800rpm, specifically, the ball milling speed is 100rpm, 200rpm, 300rpm, 400rpm, 500rpm, 600rpm, 700rpm or 800rpm. In order to achieve a better dispersion effect, the ball milling speed can be 200 rpm. Optionally, the small balls in the ball mill can be zirconia balls, and their diameter can be 1 to 10 mm. Specifically, the diameter of the zirconia balls can be 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm or 10 mm.
[0046] S103: introducing an inert gas into the target mixture, and then performing a drying process to obtain a composite positive electrode material.
[0047] In an exemplary embodiment, the temperature of the inert gas introduced is 50° C. to 700° C. Specifically, the temperature of the inert gas introduced is 50° C., 150° C., 250° C., 350° C., 450° C., 550° C., 650° C. or 700° C. In order to achieve a better drying effect, the temperature of the inert gas can be 300 to 500° C.
[0048] By using high-temperature inactive airflow for drying, the problems of long drying time and large electrolyte particles in ordinary ovens are avoided, the process efficiency is improved, and full contact between the solid electrolyte and the active material is ensured.
[0049] In an exemplary embodiment, the inert gas flow rate is 10m / s to 30m / s; the inert gas introduction time is 1s to 30s. Specifically, the inert gas flow rate is 10m / s, 15m / s, 20m / s, 25m / s or 30m / s; the inert gas introduction time is 1s, 5s, 10s, 15s, 20s, 25s or 30s. Optionally, the inert gas introduction time can be set to 30m / s and the introduction time is 10s to achieve a better drying effect.
[0050] In the embodiment of the present application, the inert gas may include but is not limited to at least one of nitrogen, helium, argon, and carbon dioxide.
[0051] This application mixes the positive electrode active material, solid electrolyte and solvent in a certain proportion, and evenly disperses them by ball milling to refine the electrolyte, and evenly coats a layer of sulfide solid electrolyte on the positive electrode active material. The solvent in the slurry is removed by high-temperature inactive gas, which avoids the problems of long drying time in ordinary ovens, growth of solid electrolyte particle size during the drying process, reduction of contact sites with the positive electrode active material, and obstruction of lithium ion migration. This method is more convenient and flexible, the coating effect is more uniform, and this method can increase the positive electrode active material loading to more than 90%, which is conducive to improving the energy density of all-solid-state batteries.
[0052] The technical effects of this application are described below with specific embodiments:
[0053] Example 1
[0054] A method for preparing a composite positive electrode material of Example 1 is provided, specifically, the sulfide solid electrolyte LPSC (i.e., Li6PS5C l), the positive electrode active material NCM, and Super P are weighed according to a mass ratio of 2:97:1, and xylene is added to prepare a mixture with a solid content of 20%.
[0055] Zirconia beads with a diameter of 1 mm were added, and the ball-to-material ratio was adjusted to 10:1. The composite positive electrode slurry was obtained after ball milling at 200 rpm for 5 h.
[0056] After nitrogen gas at 300° C. was introduced into the slurry at a flow rate of 30 m / s for 10 seconds, a composite positive electrode material of nano-scale LPSC coated with NCM was obtained.
[0057] A comparative example 1 is also provided. The preparation method of the composite positive electrode material of comparative example 1 can be specifically as follows: after weighing the sulfide solid electrolyte LPSC, the positive electrode active material NCM, and Super P according to a mass ratio of 2:97:1, adding xylene to prepare a mixture with a solid content of 20%, directly grinding and mixing the mixture manually, and then directly drying the mixed slurry to obtain the composite positive electrode material corresponding to comparative example 1.
[0058] For follow-up, please see Figure 2 and 3 , Figure 2 is a scanning electron microscope image corresponding to an exemplary embodiment 1; Figure 3 This is an exemplary scanning electron microscope image corresponding to Comparative Example 1, which can be compared Figure 2 and Figure 3 The composite positive electrode of Example 1 obtained by adopting this scheme has a layer of nano-scale sulfide solid electrolyte material uniformly coated on the surface of the positive electrode active material. Compared with the composite positive electrode obtained by artificial mixing (i.e., Comparative Example 1), the material dispersion is more uniform, and the contact between the solid electrolyte and the positive electrode active material is more sufficient. Combined with the electrochemical properties in the subsequent Table 1, it can be seen that the composite positive electrode material uniformly coated with the solid electrolyte helps to solve the problem of excessive interface impedance, has a higher capacity, and has a higher first efficiency, thereby improving battery performance.
[0059] Example 2
[0060] A method for preparing a composite positive electrode material of Example 2 is provided, specifically, the sulfide solid electrolyte LPSC, the positive electrode active material NCA, and the carbon nanotubes are weighed in a mass ratio of 7:92:1, and heptane is added to prepare a mixture with a solid content of 30%.
[0061] Zirconia beads with a diameter of 1 mm were added, and the ball-to-material ratio was adjusted to 10:1. The composite positive electrode slurry was obtained after ball milling at 200 rpm for 3 h.
[0062] After argon gas at 500° C. was introduced into the slurry at a flow rate of 30 m / s and maintained for 10 seconds, a composite positive electrode material of nano-scale LPSC coated with NCA was obtained.
[0063] A comparative example 2 is also provided. The preparation method of the composite positive electrode material of comparative example 2 can be specifically as follows: after weighing the sulfide solid electrolyte LPSC, the positive electrode active material NCA, and the carbon nanotubes in a mass ratio of 7:92:1, adding heptane to prepare a mixture with a solid content of 30%, directly grinding and mixing the mixture manually, and then directly drying the mixed slurry to obtain the composite positive electrode material corresponding to comparative example 2.
[0064] Example 3
[0065] A method for preparing a composite positive electrode material of Example 1 is provided, specifically, by preparing a sulfide solid electrolyte LGPS (i.e., Li 10 GeP2S 12 ), the positive electrode active material LFP and graphene were weighed in a mass ratio of 1:98:1, and benzyl acetate was added to prepare a mixture with a solid content of 25%.
[0066] Zirconia beads with a diameter of 1 mm were added, and the ball-to-material ratio was adjusted to 10:1. The composite positive electrode slurry was obtained after ball milling at 200 rpm for 5 h.
[0067] After carbon dioxide at 400° C. was introduced into the slurry at a flow rate of 30 m / s and maintained for 10 seconds, a composite positive electrode material of nanoscale LGPS coated with LFP was obtained.
[0068] A comparative example 3 is also provided. The preparation method of the composite positive electrode material of comparative example 3 can be specifically achieved by weighing the sulfide solid electrolyte LGPS, the positive electrode active material LFP, and the graphene according to a mass ratio of 1:98:1, adding benzyl acetate, and preparing a mixture with a solid content of 25%, and directly grinding and mixing the mixture manually. After that, the mixed slurry is directly dried to obtain the composite positive electrode material corresponding to comparative example 3.
[0069] Example 4
[0070] A method for preparing a composite positive electrode material of Example 4 is provided, specifically, the sulfide solid electrolyte 728I (i.e., Li7Si PS8), the positive electrode active material LCO, and Ketjen black are weighed in a mass ratio of 5:94:1, and isopropanol is added to prepare a mixture with a solid content of 20%.
[0071] Zirconia beads with a diameter of 1 mm were added, and the ball-to-material ratio was adjusted to 10:1. The composite positive electrode slurry was obtained after ball milling at 200 rpm for 5 h.
[0072] After helium at 300° C. was introduced into the slurry at a flow rate of 30 m / s for 10 seconds, a composite positive electrode material of nano-scale 728I coated with LCO was obtained.
[0073] A comparative example 4 is also provided. The preparation method of the composite positive electrode material of comparative example 4 can be specifically achieved by weighing the sulfide solid electrolyte 728I, the positive electrode active material LCO, and the Ketjen black according to a mass ratio of 5:94:1, adding isopropanol to prepare a mixture with a solid content of 20%, and directly grinding and mixing the mixture manually. After that, the mixed slurry is directly dried to obtain the composite positive electrode material corresponding to comparative example 4.
[0074] Example 5
[0075] A method for preparing a composite positive electrode material of Example 5 is provided, specifically, by preparing a sulfide solid electrolyte LPS7311 (i.e., Li7P3S 11 ), the positive electrode active material LMO and carbon fiber were weighed in a mass ratio of 9:90:1, and dibutyl ether was added to prepare a mixture with a solid content of 20%.
[0076] Zirconia beads with a diameter of 1 mm were added, and the ball-to-material ratio was adjusted to 10:1. The composite positive electrode slurry was obtained after ball milling at 200 rpm for 5 h.
[0077] After nitrogen gas at 300° C. was introduced into the slurry at a flow rate of 30 m / s for 10 seconds, a composite positive electrode material of nano-scale LPS7311 coated with LMO was obtained.
[0078] A comparative example 5 is also provided. The preparation method of the composite positive electrode material of comparative example 5 can be specifically as follows: after weighing the sulfide solid electrolyte LPS7311, the positive electrode active material LMO, and the carbon fiber in a mass ratio of 9:90:1, adding dibutyl ether to prepare a mixture with a solid content of 20%, directly grinding and mixing the mixture manually, and then directly drying the mixed slurry to obtain the composite positive electrode material corresponding to comparative example 1.
[0079] Example 6
[0080] A method for preparing a composite positive electrode material of Example 6 is provided, specifically, the sulfide solid electrolyte LPSC, the positive electrode active material LRMO, and acetylene carbon black are weighed in a mass ratio of 9:90:1, and anisole is added to prepare a mixture with a solid content of 20%.
[0081] Zirconia beads with a diameter of 1 mm were added, and the ball-to-material ratio was adjusted to 10:1. The composite positive electrode slurry was obtained after ball milling at 200 rpm for 5 h.
[0082] After nitrogen gas at 300° C. was introduced into the slurry at a flow rate of 30 m / s for 10 seconds, a composite cathode material of nano-scale LPSC coated with LRMO was obtained.
[0083] A comparative example 5 is also provided. The preparation method of the composite positive electrode material of comparative example 5 can be specifically achieved by weighing the sulfide solid electrolyte LPSC, the positive electrode active material LRMO, and the acetylene carbon black according to a mass ratio of 9:90:1, adding anisole, and preparing a mixture with a solid content of 20%, and directly grinding and mixing the mixture manually. After that, the mixed slurry is directly dried to obtain the composite positive electrode material corresponding to comparative example 5.
[0084] Example 7
[0085] A method for preparing a composite positive electrode material of Example 7 is provided, specifically, the sulfide solid electrolyte LPSC, the positive electrode active material LNMO, and the carbon fiber are weighed in a mass ratio of 3:96:1, and dodecane is added to prepare a mixture with a solid content of 20%.
[0086] Zirconia beads with a diameter of 1 mm were added, and the ball-to-material ratio was adjusted to 10:1. The composite positive electrode slurry was obtained after ball milling at 200 rpm for 5 h.
[0087] After nitrogen gas at 300° C. was introduced into the slurry at a flow rate of 30 m / s for 10 s, a composite cathode material of nano-scale LPSC coated with LNMO was obtained.
[0088] A comparative example 7 is also provided. The preparation method of the composite positive electrode material of comparative example 7 can be specifically as follows: after weighing the sulfide solid electrolyte LPSC, the positive electrode active material LNMO, and the carbon fiber in a mass ratio of 3:96:1, adding dodecane to prepare a mixture with a solid content of 20%, and directly grinding and mixing the mixture manually; after that, directly drying the mixed slurry to obtain the composite positive electrode material corresponding to comparative example 7.
[0089] Example 8
[0090] A method for preparing a composite positive electrode material of Example 8 is provided, specifically, the sulfide solid electrolyte LPSC, the positive electrode active material LMP, and Super P are weighed in a mass ratio of 4:95:1, and acetone is added to prepare a mixture with a solid content of 20%.
[0091] Zirconia beads with a diameter of 1 mm were added, and the ball-to-material ratio was adjusted to 10:1. The composite positive electrode slurry was obtained after ball milling at 200 rpm for 5 h.
[0092] After nitrogen gas at 300° C. was introduced into the slurry at a flow rate of 30 m / s for 10 s, a composite cathode material of nano-scale LPSC coated with LMP was obtained.
[0093] A comparative example 8 is also provided. The preparation method of the composite positive electrode material of comparative example 8 can be specifically as follows: after weighing the sulfide solid electrolyte LPSC, the positive electrode active material LMP, and Super P according to a mass ratio of 4:95:1, adding acetone to prepare a mixture with a solid content of 20%, directly grinding and mixing the mixture manually, and then directly drying the mixed slurry to obtain the composite positive electrode material corresponding to comparative example 8.
[0094] Table 1 Electrical performance test results of examples and comparative examples
[0095]
[0096] By analyzing the first effect and first discharge capacity of each example and the corresponding comparative example in Table 1 above, it can be seen that the first effect and first discharge capacity of the composite positive electrode obtained in each example are greatly improved compared with the composite positive electrode of the corresponding comparative example. It can be seen that this scheme can prepare a composite positive electrode material uniformly coated with a solid electrolyte, which helps to solve the problem of excessive interface impedance, has a higher capacity, and a higher first effect, thereby improving battery performance.
[0097] On the other hand, the present application discloses a composite positive electrode material, which is prepared based on the above-mentioned preparation method.
[0098] The present application discloses a solid-state battery in another aspect, wherein the positive electrode of the solid-state battery adopts the above-mentioned composite positive electrode material.
[0099] The above description is only an optional embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing a composite positive electrode material, It is characterized in that include: Obtain a preset mixed solution; The preset mixed solution contains positive electrode active material, solid electrolyte, conductive carbon and solvent; Performing a dispersion process on the preset mixed solution to obtain a target mixture; An inert gas is introduced into the target mixture, and then a drying process is performed to obtain a composite positive electrode material.
2. The preparation method according to claim 1, It is characterized in that The temperature of the introduced inert gas is 50°C to 700°C.
3. The preparation method according to claim 1, It is characterized in that The inert gas has an inlet flow rate of 10 m / s to 30 m / s; The inert gas is introduced for a time of 1 second to 30 seconds.
4. The preparation method according to claim 1, It is characterized in that The step of dispersing the preset mixed solution to obtain a target mixture comprises: The preset mixed solution is dispersed by using a ball mill to obtain a target mixture.
5. The preparation method according to claim 4, It is characterized in that In the dispersion process, the ball-to-material ratio in the ball mill is 1:1 to 20:
1.
6. The preparation method according to claim 1, It is characterized in that The chemical formula of the solid electrolyte is (100-xy)Li 2 S.xP 2 S 5 ·yM m N n , wherein 0≤x<100, 0≤y<100, 0≤x+y<100, 0≤m<4, 0≤n<6, M is one or more of Li, Ge, Si, Sn, Sb, and N is at least one of Se, O, Cl, Br, and I; The positive electrode active material includes at least one of lithium iron phosphate, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel manganese oxide, lithium-rich manganese-based oxide material, lithium manganese iron phosphate, lithium cobalt oxide and lithium manganese oxide; The conductive carbon comprises at least one of Super P, carbon nanotubes, Ketjen black, carbon fiber, graphene and acetylene black; The solvent includes at least one of esters, ethers, ketones and alkanes.
7. The preparation method according to claim 1, It is characterized in that The mass ratio of the positive electrode active material, the solid electrolyte and the conductive carbon is (90-98):(9-1):
1.
8. The preparation method according to claim 1, It is characterized in that The solid content of the preset mixed solution is 10% to 70%.
9. A composite positive electrode material, It is characterized in that It is prepared based on the preparation method according to any one of claims 1 to 8.
10. A solid-state battery, It is characterized in that The positive electrode of the solid-state battery adopts the composite positive electrode material as claimed in claim 9.