Sodium-ion battery positive electrode material and preparation method thereof

By using composite flux and stepwise calcination to prepare sodium-ion battery cathode materials, the problems of cycle stability and voltage plateau instability were solved, and the electrochemical performance of the materials was improved.

CN119050343APending Publication Date: 2024-11-29SHAOXING INST OF NEW ENERGY & MOLECULAR ENG SHANGHAI JIAO TONG UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411167372.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing preparation methods result in poor cycle stability and unstable voltage plateau in P3-type sodium nickel magnesium manganese layered ternary cathode materials.

Method used

A composite flux and a stepwise calcination method were used to improve the mixing uniformity by using a fluxing agent, and a low-temperature secondary calcination was performed after water washing to repair the crystal structure and improve electrochemical stability.

Benefits of technology

It significantly improves the electrochemical platform stability and cycle stability of sodium-ion battery cathode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050343A_ABST
    Figure CN119050343A_ABST
Patent Text Reader

Abstract

The invention discloses a sodium ion battery positive electrode material and a preparation method thereof. The chemical formula of the sodium ion battery positive electrode material is Na < 2 / 3 > Ni < x > Mg < y > Mn < z > O < 2 >, wherein x + y + z = 1, 0.2 < = x < = 0.6, 0.1 < = y < = 0.5, 0.3 < = z < = 0.7; the preparation method comprises the following steps: S1, uniformly mixing a fluxing agent and a fluxing agent to obtain a composite fluxing agent; s2, weighing a sodium source, a nickel source, a magnesium source and a manganese source according to the proportion of each element in Na2 / 3NixMgyMnzO2, adding a composite fluxing agent, and uniformly mixing to form a mixed precursor; s3, carrying out primary calcination on the mixed precursor in the step S2 in an aerobic atmosphere; s4, washing and drying the product obtained in the step S3 to obtain a primary product; and S5, carrying out secondary calcination on the primary product obtained in the step S4 in an aerobic atmosphere to obtain a product with stable electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion battery positive electrode materials, in particular to a sodium ion battery positive electrode material and a preparation method thereof. Background Art

[0002] Lithium-ion batteries, with their high energy density and good cycle performance, have been gradually applied to consumer electronics, electric vehicles, and large-scale energy storage power stations, becoming the most widely used secondary battery in the field of new energy. However, the widespread use of lithium-ion batteries has also led to a shortage of lithium resources, which in turn has led to an increase in the cost of lithium-ion batteries, forcing researchers to turn their attention to metallic sodium, which has a higher content in the earth's crust and is more abundant in existing resources. As a result, sodium-ion batteries, which are easy to obtain, low-cost, and highly safe, have developed rapidly in recent years.

[0003] The specific capacity of the cathode material plays a decisive role in the energy density of the entire battery. Therefore, the cathode material of sodium-ion batteries has become a research hotspot in the field of sodium-ion batteries. Among various sodium-ion battery cathode materials, P3-type NaMnO2 is the most popular. 0.66 Ni 0.1 Mg 0.33 Mn 0.3 O σ Nickel-magnesium-manganese-sodium layered ternary cathode materials have attracted extensive attention due to their high specific capacity provided by multiple transition metal elements and their wide electrochemical stability window. However, due to some defects in the existing preparation methods, P3-type nickel-magnesium-manganese-sodium layered ternary cathode materials still have problems such as poor cycle stability and unstable voltage platform.

[0004] Therefore, there is an urgent need in the art to develop a new preparation method to prepare a P3-type sodium nickel magnesium manganate layered ternary positive electrode material with better cycle stability and electrochemical stability. Summary of the invention

[0005] In view of this, an object of the present invention is to provide a sodium ion battery positive electrode material with stable electrochemical properties and a preparation method thereof.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention provides a sodium ion battery positive electrode material, wherein the chemical formula of the sodium ion battery positive electrode material is Na 2 / 3Ni x Mg y Mn z O2;

[0008] Among them, x+y+z=1, 0.2≤x≤0.6, 0.1≤y≤0.5, 0.3≤z≤0.7.

[0009] The present invention also provides a method for preparing the above-mentioned sodium ion battery positive electrode material, comprising the following steps:

[0010] S1, mixing the flux and the fluxing agent evenly to prepare a composite flux;

[0011] S2, according to the sodium ion battery positive electrode material Na 2 / 3 Ni x Mg y Mn z The proportion of each element in O2 is weighed. Sodium source, nickel source, magnesium source and manganese source are added and mixed evenly to form a mixed precursor; wherein, x+y+z=1, 0.2≤x≤0.6, 0.1≤y≤0.5, 0.3≤z≤0.7;

[0012] S3, calcining the mixed precursor of step S2 in an oxygen atmosphere;

[0013] S4, washing and drying the product obtained in step S3 to obtain a primary product;

[0014] S5. The primary product obtained in step S4 is subjected to secondary calcination in an oxygen atmosphere to obtain the positive electrode material for a sodium ion battery.

[0015] In step S1, the fluxing agent includes any one of titanium dioxide, aluminum oxide, and calcium hydroxide.

[0016] In step S1, the flux includes sodium molybdate.

[0017] Preferably, the mass ratio of the flux to the fluxing agent is 15:1 to 8:1.

[0018] In step S2, the nickel source includes at least one of nickel hydroxide, nickel carbonate, nickel oxide, nickel chloride, nickel acetate, and nickel sulfate.

[0019] Preferably, the nickel source includes at least one of nickel hydroxide and nickel carbonate.

[0020] In step S2, the magnesium source includes at least one of magnesium hydroxide, magnesium carbonate, magnesium oxide, magnesium chloride, magnesium acetate, and magnesium sulfate.

[0021] Preferably, the magnesium source includes at least one of magnesium hydroxide and magnesium carbonate.

[0022] In step S2, the manganese source includes at least one of manganese hydroxide, manganese oxide, manganese dioxide, manganese tetraoxide, manganese carbonate, and manganese chloride.

[0023] Preferably, the manganese source includes at least one of manganese dioxide, manganese tetraoxide and manganese carbonate.

[0024] In step S2, the sodium source includes at least one of sodium hydroxide, sodium carbonate, sodium oxide, sodium chloride, sodium acetate, and sodium sulfate.

[0025] Preferably, the sodium source comprises at least one of sodium hydroxide and sodium carbonate.

[0026] In step S2, the molar ratio of the composite flux to the sodium in the sodium source is 3:2-3:8.

[0027] In step S3, the primary calcination conditions are: heating to 600-850°C at a heating rate of 1-10°C / min, and keeping warm for 24-36 hours; then cooling to 120-150°C at a cooling rate of 1-10°C / min, and naturally cooling to room temperature.

[0028] In step S5, the secondary calcination conditions are: heating to 300-550°C at a heating rate of 1-10°C / min, and keeping warm for 8-12h; then cooling to 120-150°C at a cooling rate of 1-10°C / min, and naturally cooling to room temperature to obtain the sodium ion battery positive electrode material.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] 1. The present invention adopts a composite flux as the molten salt system of the molten salt method, and enhances the melting effect by the flux, so that the sodium source, nickel source, magnesium source and manganese source are mixed more evenly in the composite molten salt system. The prepared sodium ion battery positive electrode material has a complete crystal structure and uniform particle size, which significantly improves its electrochemical stability.

[0031] 2. The present invention adopts a step-by-step calcination method, by adding a second low-temperature calcination after water washing, while removing water from the product, repairing the defects of the primary product during water washing, reducing the residual alkali on the surface of the product, and stabilizing the crystal structure of the product, which helps to obtain a product with a complete crystal structure and stable electrochemical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0033] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0034] Figure 1 The XRD spectrum of the sodium ion battery positive electrode material prepared in Example 1 of the present invention;

[0035] Figure 2Comparison of charge and discharge curves of the sodium ion battery positive electrode materials prepared in Example 1, Example 2, Example 3, Example 4 and Example 5 of the present invention;

[0036] Figure 3 The cycle performance of the sodium ion battery positive electrode materials prepared in Example 1, Example 2, Example 3, Example 4, Example 5 and Comparative Example 3 of the present invention is compared;

[0037] Figure 4 The charge and discharge curves of the sodium ion battery positive electrode materials prepared in Example 1 of the present invention and Comparative Examples 1, 2, 3 and 4 are compared. DETAILED DESCRIPTION

[0038] The present invention is described in detail below in conjunction with embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, some adjustments and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0039] Example 1

[0040] This embodiment provides a sodium ion battery positive electrode material P3 type Na 2 / 3 Ni 0.2 Mg 0.3 Mn 0.5 O2, the preparation method thereof is as follows:

[0041] Step 1, mixing a flux sodium molybdate and a fluxing agent titanium dioxide in a mass ratio of 10:1 to prepare a composite flux;

[0042] Step 2, weighing Na2CO3, Ni(OH)2, Mg(OH)2, MnO2 and a composite flux in a molar ratio of 1 / 3:0.2:0.3:0.5:0.1, and mixing them evenly to obtain a mixed precursor;

[0043] Step 3, heating the mixed precursor to 750°C in an air atmosphere at a heating rate of 2°C / min, and keeping the temperature for 30 hours; then cooling the temperature to 150°C at a rate of 3°C / min, and then naturally cooling to room temperature;

[0044] Step 4, washing the product obtained in step 3 with deionized water, and drying to obtain a primary product;

[0045] Step 5, heating the primary product obtained in step 4 to 500° C. at a heating rate of 2° C. / min in an air atmosphere, and keeping the temperature for 10 hours; then cooling the temperature to 150° C. at a rate of 3° C. / min, and then naturally cooling to room temperature to obtain the sodium ion battery positive electrode material.

[0046] Example 2

[0047] The difference between this embodiment and embodiment 1 is that in step 1, the fluxing agent is replaced with aluminum oxide, and the remaining steps are the same as in embodiment 1.

[0048] Example 3

[0049] The difference between this embodiment and embodiment 1 is that in step 1, the fluxing agent is replaced with calcium hydroxide, and the remaining steps are the same as in embodiment 1.

[0050] Example 4

[0051] The difference between this embodiment and embodiment 1 is that the calcination temperature in step 3 is 850° C., the holding time is 24 h, and the remaining steps are the same as in embodiment 1. Figure 1 The XRD spectrum of the sodium ion battery positive electrode material prepared in Example 4 of the present invention;

[0052] Example 5

[0053] The difference between this embodiment and embodiment 1 is that the calcination temperature in step 5 is 300° C. and the holding time is 12 h. The remaining steps are the same as in embodiment 1.

[0054] Comparative Example 1

[0055] The difference between Comparative Example 1 and Example 1 is that only one calcination is performed, that is, the product of Comparative Example 1 is directly obtained after washing and drying in step 4.

[0056] Comparative Example 2

[0057] The difference between Comparative Example 2 and Example 1 is that the flux sodium molybdate in step 2 is replaced by Na2SiO3, and the remaining steps are the same.

[0058] Comparative Example 3

[0059] The difference between Comparative Example 3 and Example 1 is that no fluxing agent is added, that is, the composite flux in step 2 is replaced with sodium molybdate, and the remaining steps are the same as Example 1.

[0060] Comparative Example 4

[0061] The difference between Comparative Example 4 and Example 1 is that no fluxing agent and sodium molybdate are added, and the remaining steps are the same as Example 1.

[0062] Performance test case

[0063] The sodium ion battery positive electrode materials prepared in Examples 1-5 and Comparative Examples 1-3 were subjected to electrochemical performance tests.

[0064] The positive electrode materials of each sodium ion battery were mixed with conductive carbon black and polyvinylidene fluoride binder in a mass ratio of 8:1:1, and then coated on an aluminum foil with a thickness of 20 μm. After drying, circular pole pieces with a diameter of 10 mm were punched out, and the active material loading was controlled at 3 mg / cm 2 .

[0065] The above circular electrode was used as the positive electrode, sodium metal as the negative electrode, and glass fiber as the separator. The CR2025 button cell was assembled in a glove box filled with argon (H2O and O2 contents were not higher than 0.01ppm). The electrolyte used was 1mol / LNaPF6 dissolved in a sodium ion electrolyte formed by EC / DEC / FEC. The charge and discharge cycle test was carried out on a Xinwei charge and discharge tester at a voltage range of 2-4.5V and a room temperature of 30℃.

[0066] The charge and discharge curves of the sodium ion battery positive electrode materials prepared in Examples 1 to 5 are as follows: Figure 2 shown.

[0067] The cycle performance curves of Examples 1 to 5 and Comparative Example 3 are as follows Figure 3 shown.

[0068] Comparison of the charge and discharge curves of the sodium ion battery positive electrode materials prepared in Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Example 1 Figure 4 shown.

[0069] From the performance comparison between the examples and the comparative examples, it can be seen that the electrochemical platform stability and cycle stability of the sodium ion battery positive electrode material obtained by the preparation method of the present invention are significantly improved.

[0070] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A sodium ion battery cathode material, It is characterized in that The chemical formula of the sodium ion battery positive electrode material is Na 2 / 3 Ni x Mg y Mn z O 2 ; Among them, x+y+z=1, 0.2≤x≤0.6, 0.1≤y≤0.5, 0.3≤z≤0.

7.

2. A method for preparing a positive electrode material for a sodium ion battery, It is characterized in that The steps include: S1, mixing the flux and the fluxing agent evenly to prepare a composite flux; S2, according to the sodium ion battery positive electrode material Na 2 / 3 Ni x Mg y Mn z O 2 Weigh the sodium source, nickel source, magnesium source and manganese source, add the composite flux and mix them evenly to form a mixed precursor; wherein x+y+z=1, 0.2≤x≤0.6, 0.1≤y≤0.5, 0.3≤z≤0.7; S3, calcining the mixed precursor of step S2 in an oxygen atmosphere; S4, washing and drying the product obtained in step S3 to obtain a primary product; S5. The primary product obtained in step S4 is subjected to secondary calcination in an oxygen atmosphere to obtain the positive electrode material for a sodium ion battery.

3. The preparation method according to claim 2, It is characterized in that In step S1, the fluxing agent includes any one of titanium dioxide, aluminum oxide, and calcium hydroxide; And / or, the flux comprises sodium molybdate.

4. The preparation method according to claim 2, It is characterized in that In step S1, the mass ratio of the flux to the fluxing agent is 15:1 to 8:

1.

5. The preparation method according to claim 2, It is characterized in that In step S2, the nickel source includes at least one of nickel hydroxide, nickel carbonate, nickel oxide, nickel chloride, nickel acetate, and nickel sulfate; And / or, the magnesium source includes at least one of magnesium hydroxide, magnesium carbonate, magnesium oxide, magnesium chloride, magnesium acetate, and magnesium sulfate; And / or, the manganese source includes at least one of manganese hydroxide, manganese oxide, manganese dioxide, manganese tetraoxide, manganese carbonate and manganese chloride.

6. The preparation method according to claim 2, It is characterized in that In step S2, the sodium source includes at least one of sodium hydroxide, sodium carbonate, sodium oxide, sodium chloride, sodium acetate, and sodium sulfate.

7. The preparation method according to claim 2, It is characterized in that In step S2, the molar ratio of the composite flux to the sodium in the sodium source is 3:2-3:

8.

8. The preparation method according to claim 2, It is characterized in that In step S3, the primary calcination conditions are: heating to 600-850°C at a heating rate of 1-10°C / min, and keeping warm for 24-36 hours; then cooling to 120-150°C at a cooling rate of 1-10°C / min, and naturally cooling to room temperature.

9. The preparation method according to claim 2, It is characterized in that In step S5, the secondary calcination conditions are: heating to 300-550°C at a heating rate of 1-10°C / min, and keeping warm for 8-12h; then cooling to 120-150°C at a cooling rate of 1-10°C / min, and naturally cooling to room temperature to obtain the sodium ion battery positive electrode material.