High-adhesion PP film composite current collector and preparation method thereof
By modifying the preparation method of PP film, the problem of insufficient adhesion between PP film and metal coating was solved. By using polar ethylene compounds and grafted monomers, the adhesion between PP film and metal layer was improved, and the service life of battery was extended.
Patent Information
- Application Number
- CN202411295238.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-17
- Publication Date
- 2024-11-29
AI Technical Summary
Insufficient adhesion between the PP film and the metal coating affects the cycle life of the battery.
The modified PP film preparation method involves mixing PP material with polar ethylene grafted material to form a modified PP film, and setting metal layers on both sides of the film. The polar ethylene compound and grafted monomers with different structures are atomically complexed with the metal layers to improve adhesion.
It significantly improves the adhesion between the PP film and the metal layer, and extends the battery cycle life of the composite current collector.
Smart Images

Figure BDA0005045811220000061 
Figure BDA0005045811220000062 
Figure BDA0005045811220000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite current collectors, and in particular relates to a high-adhesion PP film composite current collector and a preparation method thereof. Background Art
[0002] The composite current collector is a composite material that uses PET, PP and other raw material films as base films and deposits copper and aluminum molecules on both sides through processes such as vacuum coating. It adopts a three-layer composite structure of "metal-polymer material-metal", forms nano-scale metal on the surface of polymer PET and PP films through vacuum evaporation, magnetron sputtering and other methods, and then deposits the metal layer to be thickened to more than 1μm through water electroplating.
[0003] Common types of plastic films include PET, PE, PVC, PP, PS, PC, PI, etc. Among them, PVC, PS, and PC are toxic and difficult to recycle, and are not suitable for use as substrates. Among the remaining plastics, polyethylene has a low tensile strength and may break when curled, so it is also not suitable for use as a substrate. PET has excellent electrical insulation, creep resistance, and fatigue resistance; PI has good heat resistance, resistance to extremely low temperatures, and excellent mechanical properties. PP has good heat resistance and electrical insulation, as well as a certain tensile strength, and is considered to be the most promising base film for composite current collectors.
[0004] However, PP is a non-polar material and has poor bonding to metal coatings. When it is made into an electrode current collector, it affects the cycle life of the battery.
[0005] Therefore, how to overcome the lack of bonding strength between the non-polarity of the PP film in the current collector and the metal coating is a technical problem that needs to be solved urgently in this field.
[0006] It should be noted that the above information disclosed in this background technology section is only used to understand the background technology of the present application concept, and therefore, the above description is not considered to constitute information of the prior art. Summary of the invention
[0007] The embodiments of the present disclosure at least provide a high-adhesion PP film composite current collector and a preparation method thereof.
[0008] In the first aspect, an embodiment of the present disclosure provides a high-adhesion PP film composite current collector, comprising: a modified PP film, wherein metal layers are respectively arranged on both sides of the modified PP film; wherein the modified PP film comprises a PP material and a polar ethylene grafted material in a mass ratio of 80:20; the polar ethylene grafted material comprises a PP material, a first grafted monomer, a second grafted monomer, and an initiator.
[0009] In an optional embodiment, the first grafting monomer and the second grafting monomer include any two of maleic anhydride, GMA, hydroxyethyl acrylate, styrene p-toluenesulfonic acid, acrylamide, KH570, acrylic acid, isooctyl acrylate, butyl acrylate, hydroxypropyl methacrylate and hydroxypropyl acrylate.
[0010] In an optional embodiment, the first grafting monomer is maleic anhydride, and the second grafting monomer is any one of hydroxyethyl acrylate and hydroxypropyl acrylate; and the mass ratio of the first grafting monomer to the second grafting monomer is 5:1.
[0011] In an alternative embodiment, the initiator comprises a bis-25 initiator.
[0012] In an optional embodiment, the mass ratio of the PP material, the first grafting monomer, the second grafting monomer and the initiator in the modified PP film is 100:5:1:0.5.
[0013] In an optional embodiment, it further comprises: a blending additive; the blending additive comprises any one or a combination of two of chlorinated PP and RC glue.
[0014] In an optional embodiment, the mass ratio of the PP material, the first grafting monomer, the second grafting monomer, the initiator and the blending additive in the modified PP film is 100:5:1:0.5:1-15.
[0015] In an optional embodiment, the material of the metal layer includes any one or more combinations of aluminum, copper, nickel, titanium, silver, gold, cobalt, chromium, molybdenum, tungsten and stainless steel.
[0016] In an optional embodiment, the thickness of the modified PP film is not greater than 10 μm.
[0017] In the second aspect, the embodiments of the present disclosure also provide a method for preparing a high-adhesion PP film composite current collector as described above, comprising the following steps: step S1, grafting modification at 200°C according to the ratio to obtain a polar ethylene grafted material; step S2, blending the PP material and the polar ethylene grafted material to form a cast film to obtain a modified PP film; step S3, using the modified PP film as a base film to stack metal layers on both sides to obtain a high-adhesion PP film composite current collector.
[0018] The beneficial effect of the present invention is that the high-adhesion PP film composite current collector and its preparation method polarize the non-polar PP material by adding a polar ethylene compound, and in the compounding experiment, the second grafted monomer with different structures is simultaneously complexed with the metal layer atoms to improve the adhesion of the modified PP film. After the adhesion of the modified PP film is significantly improved, the battery cycle life of the composite current collector is also significantly extended.
[0019] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention are realized and obtained by the structures particularly pointed out in the description and claims.
[0020] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are given below for detailed description as follows. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] As used herein, the phrases "in one embodiment," "according to one embodiment," "in some embodiments," and the like generally refer to the fact that the particular feature, structure, or characteristic following the phrase may be included in at least one embodiment of the present disclosure. Therefore, a particular feature, structure, or characteristic may be included in more than one embodiment of the present disclosure, so that these phrases do not necessarily refer to the same embodiment. As used herein, the terms "example," "exemplary," and the like are used to "serve as an example, instance, or illustration." Any implementation, aspect, or design described herein as "example" or "exemplary" is not necessarily to be construed as preferred or superior to other implementations, aspects, or designs. On the contrary, the use of the terms "example," "exemplary," and the like is intended to present concepts in a concrete manner.
[0023] In this document, as used herein, expressions such as "at least one of..." when following a list of elements modify the entire list of elements rather than modifying the individual elements in the list. For example, the expression "at least one of a, b, and c" should be understood to include only a, only b, only c, both a and b, both a and c, both b and c, or all of a, b, and c.
[0024] The terms used herein are only used to describe specific exemplary configurations and are not intended to be limited. As used herein, the singular articles "one", "an" and "the" may also be intended to include plural forms, unless it is clearly indicated above that this is not the case. The terms "comprise", "include" and "have" are inclusive, and therefore specify the presence of features, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, steps, operations, elements, components and / or combinations thereof. The method steps, processes and operations described herein should not be interpreted as necessarily requiring them to be performed in the specific order discussed or shown, unless specifically identified as an execution order. Additional or alternative steps may be adopted.
[0025] The embodiment of the present disclosure provides a high-adhesion PP film composite current collector, comprising: a modified PP film, wherein metal layers are respectively arranged on both sides of the modified PP film; wherein the modified PP film comprises a PP material and a polar ethylene grafted material in a mass ratio of 80:20; the polar ethylene grafted material comprises a PP material, a first grafted monomer, a second grafted monomer, and an initiator.
[0026] In some embodiments, specifically, the first grafting monomer and the second grafting monomer include any two of maleic anhydride, GMA, hydroxyethyl acrylate, styrene p-toluenesulfonic acid, acrylamide, KH570, acrylic acid, isooctyl acrylate, butyl acrylate, hydroxypropyl methacrylate and hydroxypropyl acrylate.
[0027] In some embodiments, specifically, the first grafting monomer is maleic anhydride, the second grafting monomer is any one of hydroxyethyl acrylate or hydroxypropyl acrylate; and the mass ratio of the first grafting monomer to the second grafting monomer is 5:1.
[0028] In some embodiments, specifically, the initiator includes a bis-25 initiator.
[0029] In some embodiments, specifically, the mass ratio of the PP material, the first grafting monomer, the second grafting monomer and the initiator in the modified PP film is 100:5:1:0.5.
[0030] In some embodiments, specifically, it further includes: a blending additive; the blending additive includes any one or a combination of two of chlorinated PP and RC glue.
[0031] In some embodiments, specifically, the mass ratio of the PP material, the first grafting monomer, the second grafting monomer, the initiator and the blending additive in the modified PP film is 100:5:1:0.5:1-15.
[0032] In some embodiments, specifically, the material of the metal layer includes any one or more combinations of aluminum, copper, nickel, titanium, silver, gold, cobalt, chromium, molybdenum, tungsten and stainless steel.
[0033] In some embodiments, specifically, the thickness of the modified PP film is no more than 10 μm.
[0034] The disclosed embodiment also provides a method for preparing a high-adhesion PP film composite current collector as described above, comprising the following steps: step S1, grafting modification at 200°C according to the ratio to obtain a polar ethylene grafted material; step S2, blending the PP material and the polar ethylene grafted material to form a cast film to obtain a modified PP film; step S3, using the modified PP film as a base film to stack metal layers on both sides to obtain a high-adhesion PP film composite current collector.
[0035] Some embodiments of the present invention are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.
[0036] In some embodiments, specifically, the cast film is prepared by mixing PP material and polar ethylene grafted material in a ratio of 80:20 by mass, and the formula of the polar ethylene grafted material is as follows: 100 parts of PP, 0.5 parts of Bis-25 initiator and grafted monomer, and the grafting and granulation is carried out at 200°C.
[0037] Specifically, the mass fractions of the grafted monomers in Examples 1-13 and the properties of the composite current collectors prepared according to the aforementioned method are shown in Table 1 below.
[0038] Table 1 Examples 1-13
[0039]
[0040]
[0041] As can be seen from Table 1 above, polar vinyl compounds as grafting monomers can improve the adhesion of PP, and maleic anhydride is the best monomer.
[0042] In some embodiments, specifically, the cast film is prepared by mixing PP material and polar ethylene grafted material in a ratio of 80:20 by mass, and the formula of polar ethylene grafted material is as follows: 100 parts of PP, 5 parts of maleic anhydride, 0.5 parts of bis-25 initiator and the second grafted monomer, and the grafting and granulation is carried out at 200°C.
[0043] Specifically, the mass fraction of the second grafted monomer in Examples 14-27 and the properties of the composite current collector prepared according to the aforementioned method are shown in Table 2 below.
[0044] Table 2 Examples 14-27
[0045]
[0046]
[0047] As shown in Table 2 above, grafting the second monomer can further improve the adhesion, and the best monomer is an acrylate with a hydroxyl group, such as hydroxyethyl acrylate and hydroxypropyl acrylate. The oxygen atom on the first grafted monomer maleic anhydride can be complexed with copper atoms, but maleic anhydride is a ring structure, and the electron cloud is constrained by the ring structure and cannot be fully used for complexing with copper atoms. At the same time, affected by the steric hindrance of the ring structure, it is difficult for a copper atom to complex with two maleic anhydride molecules at the same time. All of the above reduce the complex strength between maleic anhydride and copper atoms, so it is necessary to add a polar molecule to participate in the complexation with copper atoms at the same time to enhance its complex strength. Among the second grafted monomers, hydroxyethyl / propyl acrylate performs better because the hydroxyl group can provide higher complexing force with epoxy groups, siloxy groups, ester groups, etc., and the carbon chain structure of the ethyl / propyl group makes the hydroxyl group have no steric effect. Compared with acrylic acid, acrylamide, styrene-toluenesulfonic acid, etc., it can be more freely complexed with copper atoms.
[0048] In some embodiments, specifically, the cast film is prepared by mixing PP material and polar vinyl grafted material in a ratio of 80:20 by mass, and the formula of polar vinyl grafted material is as follows: 100 parts of PP, 5 parts of maleic anhydride, 1 part of hydroxyethyl acrylate, 0.5 parts of bis-25 initiator and blending additives, and the grafting and granulation is carried out at 200°C.
[0049] Specifically, the mass fractions of the blended additives in Examples 28-38 and the properties of the composite current collectors prepared according to the aforementioned method are shown in Table 3 below.
[0050] Table 3 Examples 28-38
[0051]
[0052]
[0053] It can be seen from Table 3 above that the addition of blending additives can further improve the adhesion of the composite current collector.
[0054] Specifically, the RC glue is preferably the RC glue produced by Jiangsu Xinluda Polymer Materials Co., Ltd.
[0055] In summary, the high-adhesion PP film composite current collector and its preparation method polarize the non-polar PP material by adding polar ethylene compounds, and in the compounding experiment, the second grafted monomers with different structures are simultaneously complexed with the metal layer atoms to improve the adhesion of the modified PP film. After the adhesion of the modified PP film is significantly improved, the battery cycle life of the composite current collector is also significantly extended.
[0056] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A high adhesion PP film composite current collector, characterized in that: include: A modified PP film, wherein metal layers are respectively provided on both sides of the modified PP film; in The modified PP film comprises PP material and polar ethylene grafted material in a mass ratio of 80:20; The polar ethylene grafted material comprises PP material, a first grafted monomer, a second grafted monomer and an initiator.
2. The high adhesion PP film composite current collector according to claim 1, characterized in that: The first graft monomer and the second graft monomer include any two of maleic anhydride, GMA, hydroxyethyl acrylate, styrene p-toluenesulfonic acid, acrylamide, KH570, acrylic acid, isooctyl acrylate, butyl acrylate, hydroxypropyl methacrylate and hydroxypropyl acrylate.
3. The high adhesion PP film composite current collector according to claim 2, characterized in that: The first grafting monomer is maleic anhydride, and the second grafting monomer is any one of hydroxyethyl acrylate or hydroxypropyl acrylate; and The mass ratio of the first grafting monomer to the second grafting monomer is 5:
1.
4. The high adhesion PP film composite current collector according to claim 1, characterized in that: The initiator includes a bis-25 initiator.
5. The high adhesion PP film composite current collector according to claim 1, characterized in that: The mass ratio of the PP material, the first grafting monomer, the second grafting monomer and the initiator in the modified PP film is 100:5:1:0.
5.
6. The high adhesion PP film composite current collector according to claim 1, characterized in that: Also includes: Blending additives; The blending additive includes any one of chlorinated PP and RC glue or a combination of both.
7. The high adhesion PP film composite current collector according to claim 6, characterized in that: The mass ratio of the PP material, the first grafting monomer, the second grafting monomer, the initiator and the blending additive in the modified PP film is 100:5:1:0.5:1-15.
8. The high adhesion PP film composite current collector according to claim 1, characterized in that: The material of the metal layer includes any one or more combinations of aluminum, copper, nickel, titanium, silver, gold, cobalt, chromium, molybdenum, tungsten and stainless steel.
9. The high adhesion PP film composite current collector according to claim 1, characterized in that: The thickness of the modified PP film is not greater than 10 μm.
10. A method for preparing a high-adhesion PP film composite current collector according to any one of claims 1 to 9, characterized in that: The steps include: Step S1, grafting modification at 200° C. according to the ratio to obtain a polar ethylene grafted material; Step S2, blending the PP material and the polar ethylene grafted material to form a cast film to obtain a modified PP film; Step S3, using the modified PP film as a base film to deposit metal layers on both sides to obtain a high-adhesion PP film composite current collector.