Composite proton exchange membrane, preparation method, membrane electrode and fuel cell
By using the combination of TiO2 functionalized graphene oxide and sulfonated graphene oxide in the proton exchange membrane, the problem of low conductivity of the existing film in a low humidity environment is solved, the water absorption and conductivity of the film are improved, and the water absorption and conductivity of the film are achieved. Better performance and environmental protection.
Patent Information
- Application Number
- CN202411417690.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-11-29
AI Technical Summary
The existing proton exchange membrane has low proton conductivity in low relative humidity environments and is difficult to meet the requirements of water retention and proton conductivity at the same time. It is also sensitive to humidity, is not environmentally friendly and has high cost.
The ionomer composite proton exchange membrane co-doped with TiO2 functionalized graphene oxide and sulfonated graphene oxide is used to improve the water retention and proton conductivity of the membrane by combining modified graphene oxide and sulfonated graphene oxide.
The water absorption and proton conductivity of the composite membrane are significantly improved, the tendency of agglomeration is avoided, the hydrogen permeability coefficient is reduced, and the uniformity and proton transport ability of the membrane are improved.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to a composite proton exchange membrane, a preparation method, a membrane electrode and a fuel cell. Background Art
[0002] To date, Nafion is considered to be the most advanced proton exchange membrane (PEM) material, with a polytetrafluoroethylene (PTFE) backbone terminated by sulfonates. PTFE is hydrophobic in nature, which gives the membrane mechanical and dimensional stability. The hydrophilic sulfonic acid groups contribute to water absorption and ionic conductivity. Nafion membranes have excellent proton conductivity (0.1 S cm in a fully hydrated state). -1 ), mechanical and chemical stability, but the main disadvantages are sensitivity to moisture, environmental pollution and high cost.
[0003] In order to overcome the above disadvantages, adding hygroscopic fillers such as TiO2, CeO2, ZnO, SiO2, ZrO2, and Fe3O4 to Nafion membranes or developing alternative PEMs is an excellent solution to improve the proton conductivity of Nafion in stringent environments such as low relative humidity. However, these fillers have poor dispersion and poor proton conductivity and cannot fully improve the performance of Nafion. Summary of the invention
[0004] The present invention provides a composite proton exchange membrane, a preparation method, a membrane electrode, and a fuel cell to overcome the technical defects of the prior art that the proton exchange membrane is difficult to simultaneously meet the water retention and proton conductivity requirements. The ionomer composite proton exchange membrane co-doped with TiO2 functionalized graphene oxide and sulfonated graphene oxide of the present invention can improve the water retention of the proton exchange membrane, increase the proton transmission channels of the proton exchange membrane, and improve its proton conductivity.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] In a first aspect, the present invention provides a composite proton exchange membrane, which comprises an ionomer, and modified graphene oxide distributed in the ionomer; the modified graphene oxide comprises TiO2 functionalized graphene oxide and sulfonated graphene oxide; the mass ratio of the TiO2 functionalized graphene oxide to the sulfonated graphene oxide is (0.17-6):1;
[0007] The preparation method of the TiO2 functionalized graphene oxide comprises the following steps:
[0008] S1, mixing a titanium source and a dispersant, and allowing to stand to obtain a mixture A;
[0009] S2. reacting the mixture A with graphene oxide.
[0010] In the present invention, the mass of the modified graphene oxide may be 1-2% of the mass of the ionomer.
[0011] In the present invention, the mass ratio of the TiO2 functionalized graphene oxide to the sulfonated graphene oxide may be (0.2-5):1.
[0012]
Ionomer
[0013] In the present invention, the ionomer may be perfluorosulfonic acid resin (PFSI), sulfonated polyetheretherketone (SPEEK), sulfonated polyarylethersulfone (SPES), sulfonated polyimide (SPI) or sulfonated polybenzimidazole (SPBI).
[0014] Wherein, the perfluorosulfonic acid resin may be decalin perfluorinated ion exchange resin (Nafion).
[0015] In the present invention, the ionomer can be obtained by evaporating a commercially available ionomer solution. The evaporation method can be rotary evaporation.
[0016]
TiO2 functionalized graphene oxide
[0017] In the present invention, the TiO2 functionalized graphene oxide is a conventional material in the art, and may include graphene oxide and TiO2 distributed on the graphene oxide.
[0018] Wherein, the mass ratio of the TiO2 to the graphene oxide may be 1:30.
[0019] In the present invention, in step S1, the mixing may include the following steps: mixing the titanium source with the dispersant and adjusting the pH to 3-5. When adjusting the pH, an acid may be used for adjustment. The acid is a conventional acid in the art, such as nitric acid. The concentration of the acid may be 0.5-1 mol / L. The titanium source is a conventional organic titanium source, such as tetrabutyl orthotitanate. The dispersant may be water and / or alcohol, such as water and alcohol in a mass ratio of 1:(1-10). The alcohol is a conventional fatty alcohol in the art, such as isopropanol.
[0020] In the present invention, in step S1, the standing temperature may be 50-60°C.
[0021] In the present invention, in step S1, the standing time may be 1-3 hours.
[0022] In the present invention, in step S1, stirring can be performed during the static state. The device used for the stirring can be a magnetic stirrer.
[0023] In the present invention, the mass ratio of the titanium source to the graphene oxide may be (14-140):1.
[0024] In the present invention, in step S2, the graphene oxide can be added dropwise in the form of a graphene oxide dispersion. The method for preparing the graphene oxide dispersion may include: adding the graphene oxide to water and ultrasonically dispersing the graphene oxide. The ultrasonic dispersion time is based on complete dispersion, for example, 20-60 minutes.
[0025] In the present invention, in step S2, the reaction temperature may be 40-60°C.
[0026] In the present invention, in step S2, the reaction time is preferably sufficient to complete the reaction, for example, 18-20 hours.
[0027] In the present invention, in step S2, the reaction may be stirred. The device used for stirring may be a magnetic stirrer.
[0028] In the present invention, in step S2, the reaction may be followed by centrifugation and / or washing and / or drying. The centrifugal speed may be 10000-15000 r / min. The centrifugal time may be 5-10 min. The washing may be performed until the pH of the washing liquid no longer changes. The washing may be performed by acid washing and / or alcohol washing. The drying temperature may be 50-60° C. The drying time is based on complete drying.
[0029] In the present invention, the TiO2 functionalized graphene oxide is formed by connecting titanium dioxide and graphene oxide under the bridging effect of a titanium source.
[0030]
Sulfonated graphene oxide
[0031] In the present invention, the sulfonated graphene oxide is a conventional material in the art, and the sulfonated graphene oxide contains sulfonic acid groups.
[0032] In the present invention, the method for preparing sulfonated graphene oxide may include the following steps: reacting graphene oxide with concentrated sulfuric acid.
[0033] The mass ratio of the graphene oxide to the concentrated sulfuric acid may be 1:(1-28). The mass concentration of the concentrated sulfuric acid is conventionally selected in the art, for example, 98%.
[0034] The graphene oxide can be added dropwise in the form of a graphene oxide dispersion. The preparation method of the graphene oxide dispersion may include: adding graphene oxide to water and ultrasonically dispersing the graphene oxide. The ultrasonic dispersion time is based on complete dispersion, for example, 20-60 minutes.
[0035] The reaction temperature is preferably a temperature that can complete the reaction, for example, a conventional temperature not exceeding 100°C.
[0036] The reaction time is preferably 4-8 hours, for example 6 hours, to complete the reaction.
[0037] In certain specific embodiments, the reaction can be divided into two stages: the first 2-4 h is carried out at room temperature, and the second 2-4 h is carried out at 100°C.
[0038] The reaction may be stirred, and the stirring device may be a magnetic stirrer.
[0039] Wherein, the reaction may be followed by dilution and / or filtration and / or washing and / or drying. The dilution may be carried out by adding water 2-3 times the volume of the graphene oxide dispersion. The washing may be carried out until the pH of the washing liquid no longer changes. The drying temperature may be 40-60° C. The drying time may be 10-24 hours, for example, 12 hours, based on complete drying.
[0040] In a second aspect, the present invention provides a method for preparing the composite proton exchange membrane as described above, comprising the following steps:
[0041] The solvent is removed from the mixture; the mixture comprises the ionomer, the modified graphene oxide and the solvent.
[0042] In the present invention, the solvent is a conventional organic solvent in the art, such as N,N-dimethylformamide (DMF).
[0043] In the present invention, the ionomer may be first mixed with the solvent to form an ionomer solution. The solid content of the ionomer solution may be 1-50%.
[0044] In the present invention, the mixture may be ultrasonically treated during mixing, and the ultrasonic treatment time is based on complete dispersion, for example, 20-60 minutes.
[0045] In the present invention, the temperature during the removal of the solvent may be 70-120°C.
[0046] In some specific embodiments, when removing the solvent, the temperature can be gradually increased from 70°C to 120°C.
[0047] In the present invention, the time for removing the solvent is preferably sufficient to completely remove the solvent, for example 24 hours.
[0048] In the present invention, after removing the solvent, oxidation and / or pickling and / or water washing can be performed. For the oxidation, an oxidant solution can be added for soaking. The oxidant solution can be a H2O2 solution. The concentration of the oxidant solution can be 0.5-10wt%, for example, 5wt%. During the oxidation, the ambient temperature of the soaking can be 70-80°C. During the oxidation, the soaking time can be 1-5h. During the oxidation, the oxidant solution can be a sulfuric acid solution. For pickling, an acid solution can be added for soaking. The concentration of the acid solution can be 0.5-4mol / L, for example, 1mol / L. During the pickling, the ambient temperature of the soaking can be 70-80°C. During the pickling, the soaking time can be 1h.
[0049] In a third aspect, the present invention provides a membrane electrode comprising the composite proton exchange membrane as described above.
[0050] In a fourth aspect, the present invention provides a fuel cell comprising the membrane electrode as described above.
[0051] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0052] The reagents and raw materials used in the present invention are commercially available.
[0053] The positive and progressive effects of the present invention are:
[0054] (1) The present invention co-dopes TiO2-functionalized graphene oxide and sulfonated graphene oxide into an ionomer composite proton exchange membrane, wherein the hydrophilicity of TiO2 grafted with graphene oxide improves the water retention of the composite membrane and the presence of TiO2 reduces the conductivity of graphene oxide, the sulfonic acid group of sulfonated graphene oxide increases the interface interaction between the ionomer matrix and the filler, and the presence of sulfonated graphene oxide also increases the proton transport capacity of the composite proton exchange membrane;
[0055] (2) In the present invention, the two functionalized graphene oxides avoid the tendency of graphene oxide to agglomerate, so that the uniformity of the prepared proton exchange membrane is excellent. In addition, the presence of dopants can reduce the hydrogen permeability coefficient of the proton exchange membrane. DETAILED DESCRIPTION
[0056] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0057] Example 1
[0058] A method for preparing a composite proton exchange membrane comprises the following steps:
[0059] (1) 100 mg of graphene oxide (GO) was added to 50 mL of deionized water and ultrasonically dispersed in an ice-water bath for 30 min. After dispersion, the dispersion was evenly divided into two portions of graphene oxide aqueous dispersion with equal volumes for the preparation of TiO2-functionalized graphene oxide and sulfonated graphene oxide.
[0060] (2) 7 g of tetrabutyl titanate was added to a mixture of water, isopropanol, and nitric acid. The mixture was prepared as follows: the mass ratio of isopropanol to water was 1:1, the volume was 100 mL, and the pH of the mixture was adjusted to about 3 using 1 mol / L nitric acid.
[0061] (3) The mixed solution was heated to 60° C. in an oil bath and stirred with a magnetic stirrer for 1 h. Then, 25 mL of the aqueous dispersion of graphene oxide described in step (2) was slowly added dropwise to the mixed solution, and the new mixture was stirred with a magnetic stirrer at 60° C. for 18 h. After the reaction, the reaction mixture was repeatedly centrifuged at a centrifugal speed of 15,000 r / min for 10 min.
[0062] (4) The obtained solid was washed with deionized water and ethanol for multiple times until the pH of the washing solution no longer changed. Finally, the washed solid was vacuum dried at 60° C. overnight to obtain a TiO2 functionalized graphene oxide product, wherein the mass ratio of TiO2 to graphene oxide was 1:30.
[0063] (5) Take 25 mL of graphene oxide aqueous dispersion, slowly add 1.4 g of 98 wt% concentrated sulfuric acid, place it in an oil bath, and use a magnetic stirrer to perform sulfonic acid functionalization for 6 h under condensation reflux.
[0064] (6) After the reaction in step (5) is completed, 70 mL of deionized water is added to dilute the reaction mixture. The diluted mixture is vacuum filtered using a Buchner funnel, and the residual acid in the precipitate is washed with deionized water. When the pH of the precipitate no longer changes, the precipitate is dried in a vacuum drying oven at 40° C. for 12 h to obtain a dry sulfonated graphene oxide powder.
[0065] (7) Take 10 mL (9 g) of a commercially available 5 wt% solid content ionomer solution (Nafion D2020) and perform rotary evaporation until it is in a gel state, add 10 mL of N,N-dimethylformamide (DMF), and continue to perform rotary evaporation for 10 min. Add a mixture of TiO2 functionalized graphene oxide and sulfonated graphene oxide (the mass ratio of TiO2 functionalized graphene oxide to sulfonated graphene oxide is 5:1) at a solute mass ratio of 1 wt% to the above ionomer solution, perform ultrasonic treatment for 1 h, and evenly disperse the mixture in the ionomer solution. Pour the dispersion into a mold and quickly place it in a 70°C oven, slowly raise the temperature from 70°C to 120°C, and maintain it for 24 h to evaporate the solvent to form a membrane material.
[0066] (8) The membrane material obtained in step (7) was first soaked in a 5 wt % H2O2 solution at 70°C for 1 h, then soaked in a 1 M H2SO4 solution at 80°C for 1 h, and finally soaked and cleaned with deionized water to obtain a TiO2 functionalized graphene oxide and sulfonated graphene oxide co-doped ionomer composite proton exchange membrane.
[0067] Example 2
[0068] A method for preparing a composite proton exchange membrane comprises the following steps:
[0069] (1) 100 mg of graphene oxide (GO) was added to 50 mL of deionized water and ultrasonically dispersed in an ice-water bath for 30 min. After dispersion, the dispersion was evenly divided into two portions of graphene oxide aqueous dispersion with equal volumes for the preparation of TiO2-functionalized graphene oxide and sulfonated graphene oxide.
[0070] (2) 7 g of tetrabutyl titanate was added to a mixture of water, isopropanol, and nitric acid. The mixture was prepared as follows: the mass ratio of isopropanol to water was 1:1, the volume was 100 mL, and the pH of the mixture was adjusted to about 3 using 1 mol / L nitric acid.
[0071] (3) The mixed solution was heated to 60° C. in an oil bath and stirred with a magnetic stirrer for 1 h. Then, 25 mL of the aqueous dispersion of graphene oxide described in step (2) was slowly added dropwise to the mixed solution, and the new mixture was stirred with a magnetic stirrer at 60° C. for 18 h. After the reaction, the reaction mixture was repeatedly centrifuged at a centrifugal speed of 15,000 r / min for 10 min.
[0072] (4) The obtained solid was washed with deionized water and ethanol for multiple times until the pH of the washing solution no longer changed. Finally, the washed solid was vacuum dried at 60° C. overnight to obtain a TiO2 functionalized graphene oxide product, wherein the mass ratio of TiO2 to graphene oxide was 1:30.
[0073] (5) Take 25 mL of graphene oxide aqueous dispersion, slowly add 1.4 g of 98 wt% concentrated sulfuric acid, place it in an oil bath, and use a magnetic stirrer to perform sulfonic acid functionalization for 6 h under condensation reflux.
[0074] (6) After the reaction in step (5) is completed, 70 mL of deionized water is added to dilute the reaction mixture. The diluted mixture is vacuum filtered using a Buchner funnel, and the residual acid in the precipitate is washed with deionized water. When the pH of the precipitate no longer changes, the precipitate is dried in a vacuum drying oven at 40° C. for 12 h to obtain a dry sulfonated graphene oxide powder.
[0075] (7) Take 10 mL (9 g) of a commercially available 5 wt% solid content ionomer solution (Nafion D2020) and perform rotary evaporation until it is in a gel state, add 10 mL of N,N-dimethylformamide (DMF), and continue to perform rotary evaporation for 10 min. Add a mixture of TiO2 functionalized graphene oxide and sulfonated graphene oxide (the mass ratio of TiO2 functionalized graphene oxide to sulfonated graphene oxide is 1:5) at a solute mass ratio of 1 wt% to the above ionomer solution, perform ultrasonic treatment for 1 h, and evenly disperse the mixture in the ionomer solution. Pour the dispersion into a mold and quickly place it in a 70°C oven, slowly raise the temperature from 70°C to 120°C, and maintain it for 24 h to evaporate the solvent to form a membrane material.
[0076] (8) The membrane material obtained in step (7) was first soaked in a 5 wt % H2O2 solution at 70°C for 1 h, then soaked in a 1 M H2SO4 solution at 80°C for 1 h, and finally soaked and cleaned with deionized water to obtain a TiO2 functionalized graphene oxide and sulfonated graphene oxide co-doped ionomer composite proton exchange membrane.
[0077] Example 3
[0078] A method for preparing a composite proton exchange membrane comprises the following steps:
[0079] (1) 100 mg of graphene oxide (GO) was added to 50 mL of deionized water and ultrasonically dispersed in an ice-water bath for 30 min. After dispersion, the dispersion was evenly divided into two portions of graphene oxide aqueous dispersion with equal volumes for the preparation of TiO2-functionalized graphene oxide and sulfonated graphene oxide.
[0080] (2) 7 g of tetrabutyl titanate was added to a mixture of water, isopropanol, and nitric acid. The mixture was prepared as follows: the mass ratio of isopropanol to water was 1:1, the volume was 100 mL, and the pH of the mixture was adjusted to about 3 using 1 mol / L nitric acid.
[0081] (3) The mixed solution was heated to 60° C. in an oil bath and stirred with a magnetic stirrer for 1 h. Then, 25 mL of the aqueous dispersion of graphene oxide described in step (2) was slowly added dropwise to the mixed solution, and the new mixture was stirred with a magnetic stirrer at 60° C. for 18 h. After the reaction, the reaction mixture was repeatedly centrifuged at a centrifugal speed of 15,000 r / min for 10 min.
[0082] (4) The obtained solid was washed with deionized water and ethanol for multiple times until the pH of the washing solution no longer changed. Finally, the washed solid was vacuum dried at 60° C. overnight to obtain a TiO2 functionalized graphene oxide product, wherein the mass ratio of TiO2 to graphene oxide was 1:30.
[0083] (5) Take 25 mL of graphene oxide aqueous dispersion, slowly add 1.4 g of 98 wt% concentrated sulfuric acid, place it in an oil bath, and use a magnetic stirrer to perform sulfonic acid functionalization for 6 h under condensation reflux.
[0084] (6) After the reaction in step (5) is completed, 70 mL of deionized water is added to dilute the reaction mixture. The diluted mixture is vacuum filtered using a Buchner funnel, and the residual acid in the precipitate is washed with deionized water. When the pH of the precipitate no longer changes, the precipitate is dried in a vacuum drying oven at 40° C. for 12 h to obtain a dry sulfonated graphene oxide powder.
[0085] (7) Take 10 mL (9 g) of a commercially available 5 wt% solid content ionomer solution (Nafion D2020) and perform rotary evaporation until it is in a gel state, add 10 mL of N,N-dimethylformamide (DMF), and continue to perform rotary evaporation for 10 min. Add a mixture of TiO2 functionalized graphene oxide and sulfonated graphene oxide (the mass ratio of TiO2 functionalized graphene oxide to sulfonated graphene oxide is 6:1) at a solute mass ratio of 1 wt% to the above ionomer solution, perform ultrasonic treatment for 1 h, and evenly disperse the mixture in the ionomer solution. Pour the dispersion into a mold and quickly place it in a 70°C oven, slowly raise the temperature from 70°C to 120°C, and maintain it for 24 h to evaporate the solvent to form a membrane material.
[0086] (8) The membrane material obtained in step (7) was first soaked in a 5 wt % H2O2 solution at 70°C for 1 h, then soaked in a 1 M H2SO4 solution at 80°C for 1 h, and finally soaked and cleaned with deionized water to obtain a TiO2 functionalized graphene oxide and sulfonated graphene oxide co-doped ionomer composite proton exchange membrane.
[0087] Example 4
[0088] A method for preparing a composite proton exchange membrane comprises the following steps:
[0089] (1) 100 mg of graphene oxide (GO) was added to 50 mL of deionized water and ultrasonically dispersed in an ice-water bath for 30 min. After dispersion, the dispersion was evenly divided into two portions of graphene oxide aqueous dispersion with equal volumes for the preparation of TiO2-functionalized graphene oxide and sulfonated graphene oxide.
[0090] (2) 7 g of tetrabutyl titanate was added to a mixture of water, isopropanol, and nitric acid. The mixture was prepared as follows: the mass ratio of isopropanol to water was 1:1, the volume was 100 mL, and the pH of the mixture was adjusted to about 3 using 1 mol / L nitric acid.
[0091] (3) The mixed solution was heated to 60° C. in an oil bath and stirred with a magnetic stirrer for 1 h. Then, 25 mL of the aqueous dispersion of graphene oxide described in step (2) was slowly added dropwise to the mixed solution, and the new mixture was stirred with a magnetic stirrer at 60° C. for 18 h. After the reaction, the reaction mixture was repeatedly centrifuged at a centrifugal speed of 15,000 r / min for 10 min.
[0092] (4) The obtained solid was washed with deionized water and ethanol for multiple times until the pH of the washing solution no longer changed. Finally, the washed solid was vacuum dried at 60° C. overnight to obtain a TiO2 functionalized graphene oxide product, wherein the mass ratio of TiO2 to graphene oxide was 1:30.
[0093] (5) Take 25 mL of graphene oxide aqueous dispersion, slowly add 1.4 g of 98 wt% concentrated sulfuric acid, place it in an oil bath, and use a magnetic stirrer to perform sulfonic acid functionalization for 6 h under condensation reflux.
[0094] (6) After the reaction in step (5) is completed, 70 mL of deionized water is added to dilute the reaction mixture. The diluted mixture is vacuum filtered using a Buchner funnel, and the residual acid in the precipitate is washed with deionized water. When the pH of the precipitate no longer changes, the precipitate is dried in a vacuum drying oven at 40° C. for 12 h to obtain a dry sulfonated graphene oxide powder.
[0095] (7) Take 10 mL (9 g) of a commercially available 5 wt% solid content ionomer solution (Nafion D2020) and perform rotary evaporation until it is in a gel state, add 10 mL of N,N-dimethylformamide (DMF), and continue to perform rotary evaporation for 10 min. Add a mixture of TiO2 functionalized graphene oxide and sulfonated graphene oxide (the mass ratio of TiO2 functionalized graphene oxide to sulfonated graphene oxide is 1:6) at a solute mass ratio of 1 wt% to the above ionomer solution, perform ultrasonic treatment for 1 h, and evenly disperse the mixture in the ionomer solution. Pour the dispersion into a mold and quickly place it in a 70°C oven, slowly raise the temperature from 70°C to 120°C, and maintain for 24 h to evaporate the solvent to form a membrane material.
[0096] (8) The membrane material obtained in step (7) was first soaked in a 5 wt % H2O2 solution at 70°C for 1 h, then soaked in a 1 M H2SO4 solution at 80°C for 1 h, and finally soaked and cleaned with deionized water to obtain a TiO2 functionalized graphene oxide and sulfonated graphene oxide co-doped ionomer composite proton exchange membrane.
[0097] Comparative Example 1
[0098] A method for preparing a composite proton exchange membrane comprises the following steps:
[0099] (1) 100 mg of graphene oxide (GO) was added to 50 mL of deionized water and ultrasonically dispersed in an ice-water bath for 30 min to obtain an aqueous dispersion of graphene oxide.
[0100] (2) 14 g of tetrabutyl titanate was added to a mixture of water, isopropanol, and nitric acid. The mixture was prepared as follows: the mass ratio of isopropanol to water was 1:1, the volume was 100 mL, and the pH of the mixture was adjusted to about 3 using 1 mol / L nitric acid.
[0101] (3) The mixed solution was heated to 60° C. in an oil bath and stirred with a magnetic stirrer for 1 h. Then, the aqueous dispersion of graphene oxide described in step (1) was slowly added dropwise to the mixed solution, and the new mixture was stirred with a magnetic stirrer at 60° C. for 18 h. After the reaction, the reaction mixture was repeatedly centrifuged at a centrifugal speed of 15,000 r / min for 10 min.
[0102] (4) The obtained solid was washed with deionized water and ethanol for multiple times until the pH of the washing solution no longer changed. Finally, the washed solid was vacuum dried at 60° C. overnight to obtain a TiO2 functionalized graphene oxide product, wherein the mass ratio of TiO2 to graphene oxide was 1:30.
[0103] (5) Take 10 mL (9 g) of a commercially available 5 wt% solid content ionomer solution (Nafion D2020) and perform rotary evaporation until it is in a gel state, add 10 mL of N,N-dimethylformamide (DMF), and continue to perform rotary evaporation for 10 min. Add 1 wt% TiO2 functionalized graphene oxide to the above ionomer solution, perform ultrasonic treatment for 1 h, and evenly disperse the mixture in the ionomer solution. Pour the dispersion into a mold and quickly place it in a 70°C oven, slowly raise the temperature from 70°C to 120°C, and maintain it for 24 h to evaporate the solvent to form a membrane material.
[0104] (6) The membrane material obtained in step (7) was first soaked in 5wt% H2O2 solution at 70°C for 1h, then soaked in 1M H2SO4 at 80°C for 1h, and finally soaked and cleaned with deionized water to obtain a TiO2 functionalized graphene oxide ionomer composite proton exchange membrane.
[0105] Comparative Example 2
[0106] A method for preparing a composite proton exchange membrane comprises the following steps:
[0107] (1) 100 mg of graphene oxide (GO) was added to 50 mL of deionized water and ultrasonically dispersed in an ice-water bath for 30 min to obtain an aqueous dispersion of graphene oxide.
[0108] (2) Slowly add 1.4 g of 98 wt% concentrated sulfuric acid to the aqueous dispersion of graphene oxide obtained in step (1), place it in an oil bath, and use a magnetic stirrer to perform sulfonic acid functionalization for 6 h under condensation reflux.
[0109] (3) After the reaction in step (2) is completed, 140 mL of deionized water is added to dilute the reaction mixture. The diluted mixture is vacuum filtered using a Buchner funnel, and the residual acid in the precipitate is washed with deionized water. When the pH of the precipitate no longer changes, the precipitate is dried in a vacuum drying oven at 40° C. for 12 h to obtain a dry sulfonated graphene oxide powder.
[0110] (4) Take 10 mL (9 g) of a commercially available 5 wt% solid content ionomer solution (Nafion D2020) and perform rotary evaporation until it is in a gel state, add 10 mL of N,N-dimethylformamide (DMF), and continue to perform rotary evaporation for 10 min. Add a 1 wt% sulfonated graphene oxide mixture to the above ionomer solution, perform ultrasonic treatment for 1 h, and evenly disperse the mixture in the ionomer solution. Pour the dispersion into a mold and quickly place it in a 70°C oven, slowly raise the temperature from 70°C to 120°C, and maintain it for 24 h to evaporate the solvent to form a membrane material.
[0111] (5) The membrane material obtained in step (4) was first soaked in 5 wt % H2O2 solution at 70°C for 1 h, then soaked in 1 M H2SO4 at 80°C for 1 h, and finally soaked and cleaned with deionized water to obtain a sulfonated graphene oxide ionomer composite proton exchange membrane.
[0112] Comparative Example 3
[0113] Compared with Example 1, the only difference is that the mass of TiO2 functionalized graphene oxide is replaced by titanium dioxide-graphene oxide prepared by in-situ loading. The specific method is as follows: comprising the following steps:
[0114] (1) 100 mg of graphene oxide (GO) was added to 50 mL of deionized water and ultrasonically dispersed in an ice-water bath for 30 min. After dispersion, the dispersion was evenly divided into two equal volumes of graphene oxide aqueous dispersion for the preparation of titanium dioxide-graphene oxide and sulfonated graphene oxide.
[0115] (2) Add 7 g of titanium sulfate to 25 ml of graphene oxide aqueous solution, stir magnetically for 20 min, pour the resulting mixture into a reactor, place it in a vacuum oven at 90-100 ° C for 2-3 h, and after the reaction, wash the reaction product with deionized water and anhydrous ethanol several times until there is no SO4 2- The product was detected and then dried at 120° C. to obtain dry anatase titanium dioxide-graphene oxide powder.
[0116] (3) Take 25 mL of a uniform aqueous dispersion of graphene oxide, slowly add 1.4 g of 98 wt% concentrated sulfuric acid, place it in an oil bath, and use a magnetic stirrer to perform sulfonic acid functionalization for 6 h under condensation reflux.
[0117] (4) After the reaction in step (3) is completed, 70 mL of deionized water is added to dilute the reaction mixture. The diluted mixture is vacuum filtered using a Buchner funnel, and the residual acid in the precipitate is washed with deionized water. When the pH of the precipitate no longer changes, the precipitate is dried in a vacuum drying oven at 40° C. for 12 h to obtain a dry sulfonated graphene oxide powder.
[0118] (5) Take 10 mL (9 g) of a commercially available 5 wt% solid content ionomer solution (Nafion D2020) and perform rotary evaporation until it is in a gel state, add 10 mL of N,N-dimethylformamide (DMF), and continue to perform rotary evaporation for 10 min. Add a mixture of TiO2 graphene oxide and sulfonated graphene oxide (the mass ratio of TiO2 graphene oxide to sulfonated graphene oxide is 5:1) at a solute mass ratio of 1 wt% to the above ionomer solution, perform ultrasonic treatment for 1 h, and evenly disperse the mixture in the ionomer solution. Pour the dispersion into a mold and quickly place it in a 70°C oven, slowly raise the temperature from 70°C to 120°C, and maintain for 24 h to evaporate the solvent to form a membrane material.
[0119] (6) The membrane material obtained in step (5) was first soaked in 5wt% H2O2 solution at 70°C for 1h, then soaked in 1M H2SO4 at 80°C for 1h, and finally soaked and cleaned with deionized water to obtain a TiO2 graphene oxide and sulfonated graphene oxide co-doped ionomer composite proton exchange membrane.
[0120] The experimental schemes of Examples 1-4 and Comparative Examples 1-3 are specifically listed in Table 1-2 below:
[0121] Table 1 Main raw material information in Examples and Comparative Examples
[0122]
[0123] Table 2 Main process parameters of TiO2 functionalized graphene oxide in Examples 1-4 and Comparative Examples 1-3
[0124]
[0125] Effect Example 1: Water Absorption Capacity
[0126] 1. Test objects: Composite proton exchange membranes of Examples 1-4 and Comparative Examples 1-3 and Nafion 212 proton exchange membranes
[0127] 2. Test method: Soak the proton exchange membrane in deionized water respectively. After 24 hours, take the sample out of the water, remove the excess water, and measure the weight of the wet sample W. wet , and then dried at 70 °C for 24 h, and the dry weight W was measured. dry .
[0128] The calculation formula of water absorption capacity is as follows,
[0129]
[0130] 3. Test results: The corresponding results are listed in Table 3.
[0131] Table 3 Water absorption performance test data
[0132] sample Water absorption capacity (%) sample Water absorption capacity (%) Nafion 212 39.5 Example 4 41.6 Example 1 46.2 Comparative Example 1 47.2 Example 2 42.1 Comparative Example 2 40.1 Example 3 46.8 Comparative Example 3 46.4
[0133] It can be seen from Table 3 that the water absorption capacity of Comparative Example 1 is the strongest, followed by Example 3. Since the amount of TiO2 functionalized graphene oxide added is reduced, the capacity decreases. It can be seen that the hydrophilicity of TiO2 significantly improves the water absorption / water retention of the composite membrane.
[0134] Effect Example 2: Proton Conductivity
[0135] 1. Test objects: Composite proton exchange membranes of Examples 1-4 and Comparative Examples 1-3 and Nafion 212 proton exchange membranes
[0136] 2. Test method: Shanghai Chenhua CHI660e electrochemical workstation was used for testing. The impedance value of the membrane was tested by AC impedance spectroscopy. Before the test, the membrane was soaked in deionized water to make the composite membrane fully wet. Then the cut sample membrane was placed between two layers of carbon paper, and then clamped in a homemade mold. Then the corresponding electrode wires were connected, and the lateral resistance R of the membrane was tested in an environment with a humidity of 100%. The test method adopted the three-electrode AC impedance method, the test disturbance voltage was adjusted to 5mV, and the frequency range of the impedance spectrum test was controlled to 10 -2Up to 10 6 Hz, four test temperatures are used, namely 40℃, 60℃, 80℃, and 100℃. Three samples at different positions are taken from each membrane for testing, and then the average value is taken. The proton conductivity of the sample membrane is calculated according to the following formula:
[0137]
[0138] σ: proton conductivity of the membrane;
[0139] d: thickness of the test sample film, cm;
[0140] S: The contact area between the membrane and the electrode, cm, is a fixed value of 0.503 cm -2 ;
[0141] R: The resistance value of the membrane.
[0142] 3. Test results: The test temperature was designed to be 40℃, 60℃, 80℃ and 100℃, and the relative humidity was 100%. The test results are shown in Table 4.
[0143] Table 4 Conductivity test results
[0144]
[0145] Overall, after multiple tests of conductivity under different conditions, the conductivity data in Example 2 is the best, indicating that the proton exchange membrane prepared under these conditions has the best uniformity.
Claims
1. A composite proton exchange membrane, characterized in that: It includes an ionomer, and modified graphene oxide distributed in the ionomer; the modified graphene oxide includes TiO2 functionalized graphene oxide and sulfonated graphene oxide; the mass ratio of the TiO2 functionalized graphene oxide to the sulfonated graphene oxide is (0.17-6):1; The preparation method of the TiO2 functionalized graphene oxide comprises the following steps: S1, mixing a titanium source and a dispersant, and allowing to stand to obtain a mixture A; S2. reacting the mixture A with graphene oxide.
2. The composite proton exchange membrane according to claim 1, characterized in that: The mass of the modified graphene oxide is 1-2% of the mass of the ionomer; And / or, the mass ratio of the TiO2 functionalized graphene oxide to the sulfonated graphene oxide is (0.2-5):1; And / or, the ionomer is a perfluorosulfonic acid resin, a sulfonated polyetheretherketone, a sulfonated polyarylethersulfone, a sulfonated polyimide or a sulfonated polybenzimidazole; the perfluorosulfonic acid resin is preferably a decalin perfluorinated ion exchange resin; And / or, the ionomer is obtained by evaporating an ionomer solution; the evaporation method is preferably rotary evaporation.
3. The composite proton exchange membrane according to claim 1, characterized in that: The TiO2 functionalized graphene oxide comprises graphene oxide and TiO2 distributed on the graphene oxide; the mass ratio of the TiO2 to the graphene oxide is preferably 1:30; And / or, in step S1, the mixing includes the following steps: mixing the titanium source and the dispersant, and adjusting the pH to 3-5; when adjusting the pH, it is preferably adjusted with an acid; the acid is preferably nitric acid; the concentration of the acid is preferably 0.5-1 mol / L; the titanium source is preferably tetrabutyl orthotitanate; the dispersant is preferably water and / or alcohol, for example, water and alcohol in a mass ratio of 1:(1-10); the alcohol is preferably isopropanol; And / or, in step S1, the standing temperature is 50-60°C; And / or, in step S1, the standing time is 1-3h; And / or, in step S1, stirring is performed during the standing; And / or, the mass ratio of the titanium source to the graphene oxide is (14-140):1; And / or, in step S2, the graphene oxide is added dropwise in the form of a graphene oxide dispersion; the method for preparing the graphene oxide dispersion preferably comprises: adding graphene oxide to water and ultrasonically dispersing the graphene oxide; the ultrasonic dispersion time is preferably 20-60 min; And / or, in step S2, the reaction temperature is 40-60°C; And / or, in step S2, the reaction time is 18-20h; And / or, in step S2, stirring is performed during the reaction; And / or, in step S2, the reaction is followed by centrifugation and / or washing and / or drying; the centrifugal speed is preferably 10000-15000 r / min; the centrifugal time is preferably 5-10 min; the washing is preferably performed until the pH of the washing solution no longer changes; the washing is preferably performed by acid washing and / or alcohol washing; the drying temperature is preferably 50-60°C.
4. The composite proton exchange membrane according to claim 1, characterized in that: The sulfonated graphene oxide contains sulfonic acid groups; And / or, the method for preparing sulfonated graphene oxide comprises the following steps: reacting graphene oxide with concentrated sulfuric acid.
5. The composite proton exchange membrane according to claim 4, characterized in that: The mass ratio of the graphene oxide to the concentrated sulfuric acid is 1:(1-28); the mass concentration of the concentrated sulfuric acid is preferably 98%; And / or, the graphene oxide is added dropwise in the form of a graphene oxide dispersion; the method for preparing the graphene oxide dispersion preferably comprises: adding graphene oxide to water and ultrasonically dispersing the graphene oxide; the ultrasonic dispersion time is preferably 20-60 minutes; and / or, the reaction temperature does not exceed 100°C; And / or, the reaction time is 4-8h, for example 6h; And / or, stirring is performed during the reaction; And / or, diluting and / or filtering and / or washing and / or drying are performed after the reaction; the dilution is preferably performed by adding water 2-3 times the volume of the graphene oxide dispersion; the washing is preferably performed until the pH of the washing liquid no longer changes; the drying temperature is preferably 40-60° C.; the drying time is preferably 10-24 h, for example 12 h; Preferably, the reaction is divided into two stages: the first 2-4 h is carried out at room temperature, and the last 2-4 h is carried out at 100°C.
6. A method for preparing a composite proton exchange membrane according to any one of claims 1 to 5, characterized in that: It includes the following steps: The solvent is removed from the mixture; the mixture comprises the ionomer, the modified graphene oxide and the solvent.
7. The method for preparing a composite proton exchange membrane according to claim 6, characterized in that: The solvent is N,N-dimethylformamide; And / or, the ionomer is first mixed with the solvent to form an ionomer solution; the solid content of the ionomer solution is preferably 1-50%; And / or, the mixture is subjected to ultrasound during mixing; the ultrasound time is preferably 20-60 minutes; And / or, the temperature during the removal of the solvent is 70-120°C; Preferably, when removing the solvent, the temperature can be gradually increased from 70°C to 120°C; And / or, the time for removing the solvent is 24 hours.
8. The method for preparing a composite proton exchange membrane according to claim 6, characterized in that: After removing the solvent, oxidation and / or pickling and / or water washing are performed; the oxidation is preferably performed by adding an oxidant solution for soaking, and the oxidant solution is preferably a H2O2 solution; the concentration of the oxidant solution is preferably 0.5-10wt%, for example 5wt%; during the oxidation, the soaking environment temperature is preferably 70-80°C; during the oxidation, the soaking time is preferably 1-5h; the oxidant solution is preferably a sulfuric acid solution; the pickling is preferably performed by adding an acid solution for soaking; the concentration of the acid solution is preferably 0.5-4mol / L, for example 1mol / L; during the pickling, the soaking environment temperature is preferably 70-80°C; during the pickling, the soaking time is preferably 1h.
9. A membrane electrode, characterized in that: It comprises the composite proton exchange membrane according to any one of claims 1 to 5.
10. A fuel cell, characterized in that: It comprises the membrane electrode according to claim 9.
Citation Information
Cited By
PEM water electrolysis hydrogen production membrane electrode unit, preparation method and PEM water electrolysis hydrogen production tank
CN119980292A